The sputter-system(Lesker) can be use to deposit silicon nitride by reactive sputtering with a gas mixture of Ar and N2, where N2 is the reactive gas. | The [[Specific_Process_Knowledge/Thin_film_deposition/Lesker|sputter-system(Lesker)]] can be use to deposit silicon nitride by reactive sputtering with a gas mixture of Ar and N2, where N2 is the reactive gas. | ||
We have little experience with this so any information you obtain will be welcome. | We have little experience with this so any information you obtain will be welcome. | ||
Note that it is also possible to deposit SiN by reactive sputtering in the newer [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Nitride(PC3)]] which is a dedicated chamber for metal and nitride deposition where oxygen contamination of the film will be minimized. SiO<sub>x</sub>N<sub>y</sub> may be deposited in [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Oxide(PC1)]]. These chambers also offer pulsed DC sputtering and HIPIMS (high-power impulse magnetron sputtering). | |||
Revision as of 12:16, 23 April 2020
Feedback to this page: click here
The sputter-system(Lesker) can be use to deposit silicon nitride by reactive sputtering with a gas mixture of Ar and N2, where N2 is the reactive gas.
We have little experience with this so any information you obtain will be welcome.
Note that it is also possible to deposit SiN by reactive sputtering in the newer Sputter-System Metal-Nitride(PC3) which is a dedicated chamber for metal and nitride deposition where oxygen contamination of the film will be minimized. SiOxNy may be deposited in Sputter-System Metal-Oxide(PC1). These chambers also offer pulsed DC sputtering and HIPIMS (high-power impulse magnetron sputtering).
Recipes on Sputter-System(Lesker) for deposition of silicon nitride
Recipes
The recipe below has been tried in the system. It is possible to change many of the parameters.
Recipe name | Target | Gun | Power [W] | Pressure [mTorr] | RF substrate Power [W] | Gas | Temperature | Deposition rate |
source 3 DC with nitrogen | Si | 3 | 90 | 4 | 10 | Ar+45%N2 | RT | ~1.7nm/min |
source 1 DC with RF bias and nitrogen | Si | 1 | 180 | 4 | No | Ar+45%N2 | RT | ~4.25nm/min |