Specific Process Knowledge/Thin film deposition/ALD Picosun R200/AZO deposition using ALD: Difference between revisions
Line 380: | Line 380: | ||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | |||
<b>Evgeniy Shkondin, DTU Danchip, 2015-2016.</b> | |||
<br clear="all" /> | |||
<br clear="all" /> | |||
==Morphology of deposited AZO layers== | |||
The surface morphology of deposited 100 nm ZnO/AZO thin films has been analyzed by [[Specific_Process_Knowledge/Characterization/SEM:_Scanning_Electron_Microscopy|scanning electron microscopy]] and [[Specific_Process_Knowledge/Characterization/AFM:_Atomic_Force_Microscopy|atomic force microscopy]]. | |||
===SEM morphology=== | |||
[[image:AZO_SEM_morphy_eves17032017.jpg|627x424px|left|thumb|SEM investigation of surfaces morphology for samples with dfferent doping levels and growth temperature. "D" doping level corresponds to recipes number: D20 means recipe <em>AZO 20T</em> etc.]] | |||
<br clear="all" /> | |||
===AFM morphology=== | |||
[[image:AZO_AFM_morphy_eves17032017.jpg|627x424px|left|thumb|AFM investigation of surfaces morphology for samples with different doping levels and growth temperatures. "D" doping level corresponds to recipes number: D20 means recipe <em>AZO 20T</em> etc.]] | |||
<br clear="all" /> | |||
AFM inspections of deposited ZnO/AZO films D10-D35 at 250 <sup>o</sup>C reveals a surface roughness of approx. 2 nm RMS, which slightly decreases with increasing Al content in the films. In case of D10, the Al<sup>2</sup>O<sup>3</sup> phase dominates and it result in a roughness below the acceptable detection value. The AZO films deposited at 250 <sup>o</sup>C tend to obtain a cylindrical morphology, which can be related to preferred (002) ZnO crystal orientation growth. | |||
<br clear="all" /> | <br clear="all" /> |
Revision as of 18:01, 17 March 2017
AZO can be deposited in a temperature window 150 - 250 oC. Physical and optical properties are strongly corelated with deposition temperture and Al doping concentration. All results shown on this page have been obtained using the Si(100) wafers with native oxide as substrates:
Al-doped ZnO (AZO) deposition overview
The deposition rate for AZO depends on the temperature and doping concentration, see figures that illustrate AZO growth below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
Evgeniy Shkondin, DTU Danchip, 2015-2016.
Al-doped ZnO (AZO) standard recipes
Recipe: AZO 20T
(Number 20 means doping level "D": 19 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 19 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 19 = 3.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = 4.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 25T
Number 25 means doping level "D": 14 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 24 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 24 = 4.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = 5.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 30T
(Number 30 means doping level "D": 29 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 29 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 29 = 5.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = 6.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 35T
(Number 35 means doping level "D": 34 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 34 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 34 = 6.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = 7.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
XPS investigation of AZO thin films
XPS profiles for AZO has been obtained using XPS-ThermoScientific equipment.
- XPS Investigation of AZO layers.
Typical survey scan of AZO/ZnO. b) High resolution scan of the Al 2p region for AZO/ZnO samples prepared at 250 oC c) Measured Al cocncentration in AZO films prepared at three temperatures: 150 oC, 200 oC and 250 oC. d) Deviation of the measured Al at.% concentaration from the theoretical estimation in case of 250 oC deposition temperature. Theoretical estimation can be calculated using following formula: , where GPCAl2O3 and GPCZnO are growth-per-cycle of Al2O3 and ZnO at given deposition temperature, respectively. "n" is a doping level: 05, 10, 15, 20 etc.
Recipes | 150 oC. Al at.% Concentration mesured using (XPS) | 200 oC. Al at.% Concentration mesured using (XPS) | 250 oC. Al at.% Concentration mesured using (XPS) |
---|---|---|---|
ZnOT (no doping) | 0 | 0 | 0 |
AZO 05T | 30.45 | not measured | not measured |
AZO 10T | 9.89 | 11.84 | 25.23 |
AZO 15T | 5.52 | 6.16 | 12.82 |
AZO 20T | 4.41 | 4.35 | 7.93 |
AZO 25T | 3.41 | 3.61 | 5.82 |
AZO 30T | 2.62 | 3.18 | 4.73 |
AZO 35T | not measured | not measured | 3.98 |
Evgeniy Shkondin, DTU Danchip, 2015-2016.
Morphology of deposited AZO layers
The surface morphology of deposited 100 nm ZnO/AZO thin films has been analyzed by scanning electron microscopy and atomic force microscopy.
SEM morphology
AFM morphology
AFM inspections of deposited ZnO/AZO films D10-D35 at 250 oC reveals a surface roughness of approx. 2 nm RMS, which slightly decreases with increasing Al content in the films. In case of D10, the Al2O3 phase dominates and it result in a roughness below the acceptable detection value. The AZO films deposited at 250 oC tend to obtain a cylindrical morphology, which can be related to preferred (002) ZnO crystal orientation growth.
Evgeniy Shkondin, DTU Danchip, 2015-2016.