Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test: Difference between revisions

From LabAdviser
Pevo (talk | contribs)
No edit summary
Pevo (talk | contribs)
No edit summary
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=


The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
Line 8: Line 6:
The oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.
The oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.


====Oxidation parameters====
==Oxidation parameters==


'''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
'''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"

Revision as of 09:48, 12 August 2015

The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.

At the acceptance test a dry oxide layers was grown on a boat of 150 mm wafers. The oxide growth was repeated three times

The oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.

Oxidation parameters

Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"

Oxidation time: 80 min

Oxidation temperature: 1050 oC (all temoperature zones)

O2 flow: 1 slm

The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace.

Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points on each wafer using the M-2000V ellipsometer.

Results

Oxide thickness

Date Wafer 4 Wafer 16 Wafer 28 Center point only
Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%] Average oxide thickness [nm] St. deviation Non-uniformity [%]
Run 1 28-01-2015 109.7 1.0 1.7 107.7 0.9 1.1 106.5 0.8 1.2 107.0 2.1 1.9
Run 2 28-01-2015 107.3 1.7 2.4 105.0 1.4 1.7 107.3 0.7 0.9 105.7 1.0 0.9
Run 3 30-01-2015 103.6 0.8 1.1 102.6 0.6 1.2 102.2 0.6 1.1 102.9 1.0 1.0
Average 106.9 1.2 1.7 105.1 1.0 1.3 105.3 0.7 1.1 105.2 1.4 1.3


Run-to-run
Average oxide thickness [nm] St. deviation Non-uniformity [%]
105.2 2.1 2.0


Refractive index

Date Wafer 4 Wafer 16 Wafer 28 Center point only
Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%] Average refractive index St. deviation Non-uniformity [%]
Run 1 28-01-2015 1.46 0.00 0.04 1.46 0.00 0.07 1.46 0.00 0.06 1.4609 0.0004 0.0230
Run 2 28-01-2015 1.46 0.00 0.09 1.46 0.00 0.17 1.44 0.01 0.69 1.4561 0.0094 05873
Run 3 30-01-2015 1.46 0.00 0.06 1.46 0.00 0.05 1.46 0.00 0.07 1.4602 0.0004 0.0291
Average 1.46 0.00 0.06 1.46 0.00 0.10 1.46 0.00 0.27 1.46 0.00 0.21


Run-to-run
Average refractive index St. deviation Non-uniformity [%]
1.4591 0.0026 0.1637