The ALD window for depostion of aluminium oxide ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes.  
The ALD window for depostion of aluminium dioxide (Al<sub>2</sub>O<sub>3</sub>) ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes.  


All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers with native oxide:
All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers with native oxide:


====Al<sub>2</sub>O<sub>3</sub> standard recipe====


<b>Recipe</b>: AL2O3
<b>Recipe</b>: AL2O3
Line 32: Line 33:
|}
|}


===TiO<sub>2</sub> deposition rates===


The deposition rate for Al<sub>2</sub>O<sub>3</sub> depends on the temperature, see the graph below.   
The deposition rate for Al<sub>2</sub>O<sub>3</sub> depends on the temperature, see the graph below.   
Line 50: Line 53:
image:ALD Al2O3 grow rate 350C.jpg| Temperature 350 <sup>o</sup>C.
image:ALD Al2O3 grow rate 350C.jpg| Temperature 350 <sup>o</sup>C.
</gallery>
</gallery>


Evgeniy Shkondin, DTU Danchip, February-March 2014.
Evgeniy Shkondin, DTU Danchip, February-March 2014.

Revision as of 11:52, 3 July 2015

Feedback to this page: click here


The ALD window for depostion of aluminium dioxide (Al2O3) ranges from 150 oC to 350 oC. XPS measurements shows that at temperatures below 150 oC the Al2O3 layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 oC the TMA decomposes.

All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers with native oxide:

Al2O3 standard recipe

Recipe: AL2O3

Temperature: 150 oC - 350 oC

TMA H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.1 s
Purge time 3.0 s 4.0 s


TiO2 deposition rates

The deposition rate for Al2O3 depends on the temperature, see the graph below.

Al2O3 deposition rate as function of temperature.


In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.