Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
Line 165: Line 165:
{| border="2" cellspacing="2" cellpadding="3"
{| border="2" cellspacing="2" cellpadding="3"
!Typical results
!Typical results
!Si mask STS result
!Si mask non-confirmed result
!Si mask DANCHIP result
!Si mask DANCHIP result
!Al mask STS result
!Al mask non-confirmed result
!Al mask DANCHIP result
!Al mask DANCHIP result
!Thin Al mask STS result
!Thin Al mask non-confirmed result
!Thin Al mask DANCHIP result
!Thin Al mask DANCHIP result
|-
|-

Revision as of 12:40, 18 December 2007

Because the AOE is owned by Hymite and the status of the future accessibility to this equipment is unknown - DANCHIP has not reserved much time to check and develop processes on the AOE.

Etching of micro structures in Silicon Oxide with photoresist or (poly)silicon as masking material

Parameter Si mask Resist mask
Coil Power [W] 1300 1000
Platen Power [W] 500 300
Platen temperature [oC] 35 0
He flow [sccm] 300 174
CF flow [sccm] 18 10
H flow [sccm] 0 8
Pressure [mTorr] 4 4


Typical results Si mask non-confirmed result Si mask DANCHIP result Resist mask non-confirmed result Resist mask DANCHIP result
Etch rate [nm/min] 500 300 280
Selectivity [:1] 20 4 3.2
Profile [o] >88 >88

Etching of micro structures in Silicon Oxide with Aluminium as masking material

Parameter Al mask
Coil Power [W] 1800
Platen Power [W] 180
Platen temperature [oC] 35
CF flow [sccm] 80
O flow [sccm] 10
Pressure [mTorr] 6


Typical results Al mask non-confirmed result Al mask DANCHIP result
Etch rate [nm/min] >500
Selectivity [:1] >50
Profile [o] >88

Etching of sub-micro structures (trenches or holes) in Silicon Oxide with (poly)silicon or Aluminium as masking material

Parameter Si mask Al mask Very thin Al mask
Coil Power [W] 1600 1100 2000
Platen Power [W] 200 500 140
Platen temperature [oC] 0 35 35
He flow [sccm] 300 50 60
CF flow [sccm] 6 26 29
H flow [sccm] 18 0 0
O flow [sccm] 0 0 16
Pressure [mTorr] 4 8 3


Typical results Si mask non-confirmed result Si mask DANCHIP result Al mask non-confirmed result Al mask DANCHIP result Thin Al mask non-confirmed result Thin Al mask DANCHIP result
Etch rate [nm/min] 200 275
Selectivity [:1] 11 >50 Should be larger than for the other Al mask recipe
Profile [o] 86 90 90