Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE: Difference between revisions
Jump to navigation
Jump to search
Line 95: | Line 95: | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
!Typical results | !Typical results | ||
!Al mask | !Al mask non-confirmed result | ||
!Al mask DANCHIP result | !Al mask DANCHIP result | ||
|- | |- | ||
Line 111: | Line 111: | ||
|- | |- | ||
|} | |} | ||
==Etching of sub-micro structures (trenches or holes) in Silicon Oxide with (poly)silicon or Aluminium as masking material== | ==Etching of sub-micro structures (trenches or holes) in Silicon Oxide with (poly)silicon or Aluminium as masking material== |
Revision as of 12:38, 18 December 2007
Because the AOE is owned by Hymite and the status of the future accessibility to this equipment is unknown - DANCHIP has not reserved much time to check and develop processes on the AOE.
Etching of micro structures in Silicon Oxide with photoresist or (poly)silicon as masking material
Parameter | Si mask | Resist mask |
---|---|---|
Coil Power [W] | 1300 | 1000 |
Platen Power [W] | 500 | 300 |
Platen temperature [oC] | 35 | 0 |
He flow [sccm] | 300 | 174 |
CF flow [sccm] | 18 | 10 |
H flow [sccm] | 0 | 8 |
Pressure [mTorr] | 4 | 4 |
Typical results | Si mask non-confirmed result | Si mask DANCHIP result | Resist mask non-confirmed result | Resist mask DANCHIP result |
---|---|---|---|---|
Etch rate [nm/min] | 500 | 300 | 280 | |
Selectivity [:1] | 20 | 4 | 3.2 | |
Profile [o] | >88 | >88 |
Etching of micro structures in Silicon Oxide with Aluminium as masking material
Parameter | Al mask |
---|---|
Coil Power [W] | 1800 |
Platen Power [W] | 180 |
Platen temperature [oC] | 35 |
CF flow [sccm] | 80 |
O flow [sccm] | 10 |
Pressure [mTorr] | 6 |
Typical results | Al mask non-confirmed result | Al mask DANCHIP result |
---|---|---|
Etch rate [nm/min] | >500 | |
Selectivity [:1] | >50 | |
Profile [o] | >88 |
Etching of sub-micro structures (trenches or holes) in Silicon Oxide with (poly)silicon or Aluminium as masking material
Parameter | Si mask | Al mask | Very thin Al mask |
---|---|---|---|
Coil Power [W] | 1600 | 1100 | 2000 |
Platen Power [W] | 200 | 500 | 140 |
Platen temperature [oC] | 0 | 35 | 35 |
He flow [sccm] | 300 | 50 | 60 |
CF flow [sccm] | 6 | 26 | 29 |
H flow [sccm] | 18 | 0 | 0 |
O flow [sccm] | 0 | 0 | 16 |
Pressure [mTorr] | 4 | 8 | 3 |
Typical results | Si mask STS result | Si mask DANCHIP result | Al mask STS result | Al mask DANCHIP result | Thin Al mask STS result | Thin Al mask DANCHIP result |
---|---|---|---|---|---|---|
Etch rate [nm/min] | 200 | 275 | ||||
Selectivity [:1] | 11 | >50 | Should be larger than for the other Al mask recipe | |||
Profile [o] | 86 | 90 | 90 |