Specific Process Knowledge/Thin film deposition/Deposition of Nickel/Electroplating of nickel: Difference between revisions
Line 31: | Line 31: | ||
![[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel/Electroplating_of_nickel|DCHimm18-12]] | ![[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel/Electroplating_of_nickel|DCHimm18-12]] | ||
|- | |- | ||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Charge [Ah] | |||
|18 | |||
|18 | |||
|18 | |||
|18 | |||
|- | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
Line 40: | Line 47: | ||
|320-330 µm | |320-330 µm | ||
|- | |- | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
Line 69: | Line 75: | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! | !Process comments | ||
| | |||
Fastest possible process (maximum allowable current). One must accept the following (often unwanted) material properties: high stress levels in deposited nickel, high roughness, quite ductile nickel. | |||
| | |||
A fast program that allows one to produce two samples in a normal working day. Similar material properties as stated for the 3 hour process, although slightly less 'severe'. | |||
| | | | ||
A compromise between desired material properties (hardness, ductility, roughness) and process time. Will result in a sample that will be useful for most standard injection molding processes. | |||
| | | | ||
A slower process that in return results in lower roughness and stronger mechanical properties. A good choice for shims that will be used with 'harsh' injection molding parameters (high temperatures and high pressures). | |||
|- | |- | ||
Revision as of 16:09, 27 May 2013
Electroplating of nickel: Danchip standard processes
Feedback to this page: click here
DTU Danchip Standard Programs
Four different Danchip standard programs have been made. They have all been made to fabricate nickel shims for use in the polymer injection molder at Danchip. For this purpose a nickel thickness of around 320-330 µm is required. By experimentation it has been found that the required charge for this sample thickness is 18,0 Ah. The only difference between the four different standard programs are the time required for depositing the nickel. The four different standard programs deposit 320-330 µm of nickel in about 3, 4, 6 and 12 hours respectively.
The following figure shows the current profile during the first 2 hours of the programs:
As can be seen from the illustration the first 30 minutes of all standard processes are identical. All processes use a slow ramping of the current. This is to make sure that some material is deposited which can conduct a higher current. Starting a plating process at several amperes is very likely to damage the sample (and possibly the sample holder) because the seed layer (usually 75-120 nm thick) cannot support that high currents.
The Standard programs are named using the following convention: DCHimmXX-YY where DCH indicates it's a process developed by Danchip, imm that is a process developed for producing samples for the injection molding machine, XX denotes the charge in Ah (Ampere-hours) and YY denotes the approximate process time in hours.
Comparison of standard processes
DCHimm18-03 | DCHimm18-04 | DCHimm18-06 | DCHimm18-12 | |
---|---|---|---|---|
Charge [Ah] | 18 | 18 | 18 | 18 |
Expected nickel thickness | 320-330 µm | 320-330 µm | 320-330 µm | 320-330 µm |
Maximum current [A] |
7,5 |
5,5 |
3,5 |
1,5 |
Process time [hh:mm:ss] |
02:41:01 |
xx:xx:xx |
xx:xx:xx |
12:16:01 |
Process comments |
Fastest possible process (maximum allowable current). One must accept the following (often unwanted) material properties: high stress levels in deposited nickel, high roughness, quite ductile nickel. |
A fast program that allows one to produce two samples in a normal working day. Similar material properties as stated for the 3 hour process, although slightly less 'severe'. |
A compromise between desired material properties (hardness, ductility, roughness) and process time. Will result in a sample that will be useful for most standard injection molding processes. |
A slower process that in return results in lower roughness and stronger mechanical properties. A good choice for shims that will be used with 'harsh' injection molding parameters (high temperatures and high pressures). |
Allowed materials |
|
|
Example
Feedback to this page: click here
Deposition of silicon nitride
Deposition of silicon nitride can be done with either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stiochiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace, and PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well.
- Nitride deposition using PECVD (or oxynitride)
Comparison of LPCVD and PECVD for silicon nitride deposition
LPCVD | PECVD | |
---|---|---|
Generel description | Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | Plasma Enhanced Chemical Vapour Deposition (PECVD process) |
Stoichiometry |
Si3N4: Stoichiometric nitride SRN: Silicon rich (low stress) nitride |
Silicon nitride can be doped with boron, phosphorus or germanium |
Film thickness |
Thicker nitride layers can be deposited over more runs |
|
Process temperature |
|
|
Step coverage |
|
|
Film quality |
|
|
KOH etch rate (80 oC) |
|
|
BHF etch rate |
|
|
Batch size |
Depending on what furnace you use |
Depending on what PECVD you use |
Allowed materials |
Processed wafers have to be RCA cleaned |
|