Specific Process Knowledge/Thin film deposition/Deposition of Nickel/Electroplating of nickel: Difference between revisions
Created page with "hhh" |
No edit summary |
||
Line 1: | Line 1: | ||
Electroplating of nickel: Danchip standard processes | |||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel/Electroplating_of_nickel click here]''' | |||
<br clear="all" /> | |||
== Name of processes == | |||
Four different Danchip standard programs have been made. They have all been made to fabricate nickel shims for use in the polymer injection molder at Danchip. For this purpose a nickel thickness of around 320-330 µm is required. By experimentation it has been found that the required charge for this sample thickness is 18,0 Ah. The only difference between the four different standard programs are the time required for depositing the nickel. The four different standard programs deposit 320-330 µm of nickel in about 3, 4, 6 and 12 hours respectively. | |||
The following figure shows the current profile during the first 2 hours of the programs: | |||
<br clear="all" /> | |||
==Comparison method 1 and method 2 for the process== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|Method 1]] | |||
![[Specific Process Knowledge/Thin film deposition/PECVD|Method 2]] | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Generel description | |||
|Generel description - method 1 | |||
|Generel description - method 2 | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Parameter 1 | |||
| | |||
*A | |||
*B | |||
| | |||
*A | |||
*B | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Parameter 2 | |||
| | |||
*A | |||
*B | |||
*C | |||
| | |||
*A | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Substrate size | |||
| | |||
*<nowiki>#</nowiki> small samples | |||
*<nowiki>#</nowiki> 50 mm wafers | |||
*<nowiki>#</nowiki> 100 mm wafers | |||
*<nowiki>#</nowiki> 150 mm wafers | |||
| | |||
*<nowiki>#</nowiki> small samples | |||
*<nowiki>#</nowiki> 50 mm wafers | |||
*<nowiki>#</nowiki> 100 mm wafers | |||
*<nowiki>#</nowiki> 150 mm wafers | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!'''Allowed materials''' | |||
| | |||
*Allowed material 1 | |||
*Allowed material 2 | |||
| | |||
*Allowed material 1 | |||
*Allowed material 2 | |||
*Allowed material 3 | |||
|- | |||
|} | |||
<br clear="all" /> | |||
=Example= | |||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride&action=submit click here]''' | |||
<br clear="all" /> | |||
== Deposition of silicon nitride == | |||
Deposition of silicon nitride can be done with either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stiochiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace, and PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well. | |||
*[[/Deposition of silicon nitride using LPCVD|Nitride deposition using LPCVD]] | |||
*[[/Deposition of silicon nitride using PECVD|Nitride deposition using PECVD]] (''or oxynitride'') | |||
<br clear="all" /> | |||
==Comparison of LPCVD and PECVD for silicon nitride deposition== | |||
{|border="1" cellspacing="1" cellpadding="1" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|LPCVD]] | |||
![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Generel description | |||
|Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | |||
|Plasma Enhanced Chemical Vapour Deposition (PECVD process) | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Stoichiometry | |||
| | |||
*Si<sub>3</sub>N<sub>4</sub> | |||
*SRN (only 4" nitride furnace) | |||
Si<sub>3</sub>N<sub>4</sub>: Stoichiometric nitride | |||
SRN: Silicon rich (low stress) nitride | |||
| | |||
*Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub> | |||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | |||
Silicon nitride can be doped with boron, phosphorus or germanium | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Film thickness | |||
| | |||
*Si<sub>3</sub>N<sub>4</sub>: ~50 Å - ~1400 Å | |||
*SRN: ~50 Å - ~2800 Å | |||
Thicker nitride layers can be deposited over more runs | |||
| | |||
*~40 nm - 10 µm | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Process temperature | |||
| | |||
*780 <sup>o</sup>C - 845 <sup>o</sup>C | |||
| | |||
*300 <sup>o</sup>C | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Step coverage | |||
| | |||
*Good | |||
| | |||
*Less good | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Film quality | |||
| | |||
*Deposition on both sides og the substrate | |||
*Dense film | |||
*Few defects | |||
| | |||
*Deposition on one side of the substrate | |||
*Less dense film | |||
*Incorporation of hydrogen in the film | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!KOH etch rate (80 <sup>o</sup>C) | |||
| | |||
*Expected <1 Å/min | |||
| | |||
*Dependent on recipe: ~1-10 Å/min | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!BHF etch rate | |||
| | |||
*Very low | |||
| | |||
*Very high compared the LPCVD nitride | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Batch size | |||
| | |||
*1-25 100 mm wafers | |||
*1-25 150 mm wafers (only 6" furnace) | |||
Depending on what furnace you use | |||
| | |||
*Several smaller samples | |||
*1-several 50 mm wafers | |||
*1-3 100 mm wafers | |||
*1 150 mm wafer | |||
Depending on what PECVD you use | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!'''Allowed materials''' | |||
| | |||
*Silicon | |||
*Silicon oxide | |||
*Silicon nitride | |||
*Pure quartz (fused silica) | |||
Processed wafers have to be RCA cleaned | |||
| | |||
*Silicon | |||
*Silicon oxide (with boron, phosphorous and germanium) | |||
*Silicon nitrides (with boron, phosphorous and germanium) | |||
*Pure quartz (fused silica) | |||
|- | |||
|} | |||
<br clear="all" /> |
Revision as of 15:26, 27 May 2013
Electroplating of nickel: Danchip standard processes
Feedback to this page: click here
Name of processes
Four different Danchip standard programs have been made. They have all been made to fabricate nickel shims for use in the polymer injection molder at Danchip. For this purpose a nickel thickness of around 320-330 µm is required. By experimentation it has been found that the required charge for this sample thickness is 18,0 Ah. The only difference between the four different standard programs are the time required for depositing the nickel. The four different standard programs deposit 320-330 µm of nickel in about 3, 4, 6 and 12 hours respectively.
The following figure shows the current profile during the first 2 hours of the programs:
Comparison method 1 and method 2 for the process
Method 1 | Method 2 | |
---|---|---|
Generel description | Generel description - method 1 | Generel description - method 2 |
Parameter 1 |
|
|
Parameter 2 |
|
|
Substrate size |
|
|
Allowed materials |
|
|
Example
Feedback to this page: click here
Deposition of silicon nitride
Deposition of silicon nitride can be done with either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stiochiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace, and PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well.
- Nitride deposition using PECVD (or oxynitride)
Comparison of LPCVD and PECVD for silicon nitride deposition
LPCVD | PECVD | |
---|---|---|
Generel description | Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | Plasma Enhanced Chemical Vapour Deposition (PECVD process) |
Stoichiometry |
Si3N4: Stoichiometric nitride SRN: Silicon rich (low stress) nitride |
Silicon nitride can be doped with boron, phosphorus or germanium |
Film thickness |
Thicker nitride layers can be deposited over more runs |
|
Process temperature |
|
|
Step coverage |
|
|
Film quality |
|
|
KOH etch rate (80 oC) |
|
|
BHF etch rate |
|
|
Batch size |
Depending on what furnace you use |
Depending on what PECVD you use |
Allowed materials |
Processed wafers have to be RCA cleaned |
|