''Made by Kristian Hagsted Rasmussen @ Nanotech''  
''Made by Kristian Hagsted Rasmussen @ Nanotech'' <br\>
Best recipe with respect to the etch profile and low redeposition:
Best recipe with respect to the etch profile and low redeposition:
{| border="2" cellspacing="2" cellpadding="3"  
{| border="2" cellspacing="2" cellpadding="3"  

Revision as of 10:54, 14 September 2012

Results for Si etching in the IBE

Made by Kristian Hagsted Rasmussen @ Nanotech <br\> Best recipe with respect to the etch profile and low redeposition:

Parameter Best Si etching recipe so fare
Neutalizer current [mA] 450
RF Power [W] 1200
Beam current [mA] 400
Beam voltage [V] 400
Beam accelerator voltage 400
Ar flow to neutralizer [sccm] 6.0
Ar flow to beam [sccm] 6.0
Rotation speed [rpm] 20
Stage angle [degrees] 10
Results vvv
Etch rate [nm/min] 15-30?