Revision as of 15:19, 18 July 2023

Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023

This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.

Parameter Recipe name: SiO2_ICP
Coil Power [W] 1000
Platen Power [W] 200
Platen temperature [oC] 20
C4F8 flow [sccm] 10
H2 flow [sccm] 28
Pressure [mTorr] 2.5

Results when etching a non-patterned wafer

Recipe Recipe: SIO2_ICP SIO2_ICP on stoic Nit SIO2_ICP on low-stress Nit SIO2_ICP on Si
Etch rate 121 nm/min

(18.07.2023 mfarin @ DTU nanolab)

194 nm/min

(24.05.2023 mfarin @ DTU nanolab)

190 nm/min

(24.05.2023 mfarin @ DTU nanolab)

Results when etching a patterned wafer

Material to be etched Recipe: SIO2_ICP SIO2_ICP on stoic Nit SIO2_ICP on low-stress Nit SIO2_ICP on Si
Etch rate in SiO2 155 nm/min in the center, 125nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Etch rate in resist (AZ 5214E) 108 nm/min in the center, 98nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Selectivity (SiO2:resist) 1.45
Etch rate in silicon
Profile Images SiO2 ICP.2-top-02.png

SiO2 ICP.2-top-04.png

  • More tests will be done regarding silicon and silicon nitride, since this recipe can be used for overetch.