Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions
Jump to navigation
Jump to search
Line 32: | Line 32: | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
|-style="background:DarkGray; color:White" | |-style="background:DarkGray; color:White" | ||
! | !Recipe | ||
!Recipe: SIO2_ICP | !Recipe: SIO2_ICP | ||
!SIO2_ICP on stoic Nit | !SIO2_ICP on stoic Nit |
Revision as of 15:06, 18 July 2023
Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a non-patterned wafer
Recipe | Recipe: SIO2_ICP | SIO2_ICP on stoic Nit | SIO2_ICP on low-stress Nit | SIO2_ICP on Si |
---|---|---|---|---|
Etch rate | 155 nm/min in the center, 125nm/min in the edges
(03052023 mfarin @ DTU nanolab) |
194 nm/min
(24052023 mfarin @ DTU nanolab) |
190 nm/min
(24052023 mfarin @ DTU nanolab) |
Results when etching a patterned wafer
- More tests will be done regarding silicon and silicon nitride, since this recipe can be used for overetch.