*Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023 | |||
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature. | This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature. |
Revision as of 16:48, 30 May 2023
- Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a patterned wafer
- More tests will be done regarding silicon and silicon nitride, since this recipe can be used for overetch.