Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
Line 38: | Line 38: | ||
|- | |- | ||
|Etch rate in SiO2 | |Etch rate in SiO2 | ||
|155 nm/min in the center, 125nm/min in the edges (03052023 mfarin @ DTU nanolab) | |155 nm/min in the center, 125nm/min in the edges | ||
(03052023 mfarin @ DTU nanolab) | |||
| | | | ||
|- | |- | ||
|Etch rate in resist (AZ 5214E) | |Etch rate in resist (AZ 5214E) | ||
|108 nm/min in the center, 98nm/min in the edges (03052023 mfarin @ DTU nanolab) | |108 nm/min in the center, 98nm/min in the edges | ||
(03052023 mfarin @ DTU nanolab) | |||
| | | | ||
|- | |- |
Revision as of 09:53, 24 May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a patterned wafer