This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a patterned wafer
Material to be etched | Recipe: SIO2_ICP | Testing othe etch rate in nitride |
---|---|---|
Etch rate in SiO2 | 155 nm/min in the center, 125nm/min in the edges. | |
Etch rate in resist (AZ 5214E) | 108 nm/min in the center, 98nm/min in the edges | |
Selectivity (SiO2:resist) | 1.45 | |
Etch rate in silicon | ||
Profile Images | File:SiO2 ICP.2 top 02.tifFile:SiO2 ICP.2 top 04.tif |