Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test: Difference between revisions
No edit summary |
|||
Line 4: | Line 4: | ||
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie. | The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie. | ||
At the acceptance test a dry oxide layers was grown on a boat of 150 mm wafers. The oxide growth was repeated three times | |||
The oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run. | |||
====Oxidation parameters==== | |||
'''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV" | '''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV" | ||
Line 17: | Line 20: | ||
The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace. | The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace. | ||
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured. | Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points on each wafer using the M-2000V ellipsometer. | ||
==Results== | ==Results== | ||
====Oxide thickness==== | ====Oxide thickness==== | ||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
Line 126: | Line 127: | ||
====Refractive index==== | ====Refractive index==== | ||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" |
Revision as of 10:46, 12 August 2015
THIS PAGE IS UNDER CONSTRUCTION
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
At the acceptance test a dry oxide layers was grown on a boat of 150 mm wafers. The oxide growth was repeated three times
The oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run.
Oxidation parameters
Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
Oxidation time: 80 min
Oxidation temperature: 1050 oC (all temoperature zones)
O2 flow: 1 slm
The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace.
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points on each wafer using the M-2000V ellipsometer.
Results
Oxide thickness
Date | Wafer 4 | Wafer 16 | Wafer 28 | Center point only | |||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | ||
Run 1 | 28-01-2015 | 109.7 | 1.0 | 1.7 | 107.7 | 0.9 | 1.1 | 106.5 | 0.8 | 1.2 | 107.0 | 2.1 | 1.9 |
Run 2 | 28-01-2015 | 107.3 | 1.7 | 2.4 | 105.0 | 1.4 | 1.7 | 107.3 | 0.7 | 0.9 | 105.7 | 1.0 | 0.9 |
Run 3 | 30-01-2015 | 103.6 | 0.8 | 1.1 | 102.6 | 0.6 | 1.2 | 102.2 | 0.6 | 1.1 | 102.9 | 1.0 | 1.0 |
Average | 106.9 | 1.2 | 1.7 | 105.1 | 1.0 | 1.3 | 105.3 | 0.7 | 1.1 | 105.2 | 1.4 | 1.3 |
Run-to-run | ||
---|---|---|
Average oxide thickness [nm] | St. deviation | Non-uniformity [%] |
105.2 | 2.1 | 2.0 |
Refractive index
Date | Wafer 4 | Wafer 16 | Wafer 28 | Center point only | |||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | ||
Run 1 | 28-01-2015 | 1.46 | 0.00 | 0.04 | 1.46 | 0.00 | 0.07 | 1.46 | 0.00 | 0.06 | 1.4609 | 0.0004 | 0.0230 |
Run 2 | 28-01-2015 | 1.46 | 0.00 | 0.09 | 1.46 | 0.00 | 0.17 | 1.44 | 0.01 | 0.69 | 1.4561 | 0.0094 | 05873 |
Run 3 | 30-01-2015 | 1.46 | 0.00 | 0.06 | 1.46 | 0.00 | 0.05 | 1.46 | 0.00 | 0.07 | 1.4602 | 0.0004 | 0.0291 |
Average | 1.46 | 0.00 | 0.06 | 1.46 | 0.00 | 0.10 | 1.46 | 0.00 | 0.27 | 1.46 | 0.00 | 0.21 |
Run-to-run | ||
---|---|---|
Average refractive index | St. deviation | Non-uniformity [%] |
1.4591 | 0.0026 | 0.1637 |