The ALD window for depostion of aluminium oxide ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes. | The ALD window for depostion of aluminium oxide ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes. | ||
All results shown on this page have been obtained using the "AL2O3" recipe: | All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers: | ||
Revision as of 13:24, 9 July 2014
Feedback to this page: click here
The ALD window for depostion of aluminium oxide ranges from 150 oC to 350 oC. XPS measurements shows that at temperatures below 150 oC the Al2O3 layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 oC the TMA decomposes.
All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers:
Recipe: AL2O3
Temperature: 150 oC - 350 oC
TMA | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 3.0 s | 4.0 s |
The deposition rate for Al2O3 depends on the temperature, see the graph below.
![]() |
---|
In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.
- Aluminium oxide thickness as function of number of cycles
-
Temperature 150 oC.
-
Temperature 200 oC.
-
Temperature 250 oC.
-
Temperature 300 oC.
-
Temperature 350 oC.
Evgeniy Shkondin, DTU Danchip, February-March 2014.