The ALD window for depostion of Al<sub>2</sub>O<sub>3</sub> ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes.
The deposition rate for Al<sub>2</sub>O<sub>3</sub> depends on the temperature
{| border="1" cellspacing="1" cellpadding="2"
!
[[Image:ALD window Al2O3 H2O.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 150 <sup>o</sup>C.]]
|}
Below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated.


{| border="1" cellspacing="1" cellpadding="2"  
{| border="1" cellspacing="1" cellpadding="2"  
!
!
[[Image:ALD Al2O3 grow rate 300C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 300 <sup>o</sup>C. Evgeniy Shkondin, DTU Danchip, February 2014.]]
[[Image:ALD Al2O3 grow rate 150C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 150 <sup>o</sup>C.]]
|}
|}


{| border="1" cellspacing="1" cellpadding="2"  
{| border="1" cellspacing="1" cellpadding="2"  
!
!
[[Image:ALD Al2O3 grow rate 200C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 200 <sup>o</sup>C. Evgeniy Shkondin, DTU Danchip, February 2014.]]
[[Image:ALD Al2O3 grow rate 200C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 200 <sup>o</sup>C.]]
|}
|}
{| border="1" cellspacing="1" cellpadding="2"
!
[[Image:ALD Al2O3 grow rate 250C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 250 <sup>o</sup>C.]]
|}
{| border="1" cellspacing="1" cellpadding="2"
!
[[Image:ALD Al2O3 grow rate 300C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 300 <sup>o</sup>C.]]
|}
{| border="1" cellspacing="1" cellpadding="2"
!
[[Image:ALD Al2O3 grow rate 350C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 350 <sup>o</sup>C.]]
|}
{| border="1" cellspacing="1" cellpadding="2"
!
[[Image:ALD Al2O3 grow rate 300C.jpg|300x300px|thumb|center|Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles, temperature 300 <sup>o</sup>C.]]
|}
All results above have been obtained by Evgeniy Shkondin, DTU Danchip, February-March 2014.

Revision as of 10:49, 27 March 2014

THIS PAGE IS UNDER CONSTRUCTION

The ALD window for depostion of Al2O3 ranges from 150 oC to 350 oC. XPS measurements shows that at temperatures below 150 oC the Al2O3 will be contaminated by unreacted TMA molecules, and at temperatures above 350 oC the TMA decomposes.

The deposition rate for Al2O3 depends on the temperature

Al2O3 thickness as function of number of cycles, temperature 150 oC.


Below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.

Al2O3 thickness as function of number of cycles, temperature 150 oC.


Al2O3 thickness as function of number of cycles, temperature 200 oC.


Al2O3 thickness as function of number of cycles, temperature 250 oC.


Al2O3 thickness as function of number of cycles, temperature 300 oC.


Al2O3 thickness as function of number of cycles, temperature 350 oC.


Al2O3 thickness as function of number of cycles, temperature 300 oC.

All results above have been obtained by Evgeniy Shkondin, DTU Danchip, February-March 2014.