Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions
Jump to navigation
Jump to search
(9 intermediate revisions by the same user not shown) | |||
Line 28: | Line 28: | ||
|} | |} | ||
====Results | ====Results with a ''non-patterned wafer''==== | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
|-style="background:DarkGray; color:White" | |-style="background:DarkGray; color:White" | ||
! | !Recipe | ||
!Recipe: SIO2_ICP | !Recipe: SIO2_ICP | ||
!SIO2_ICP on stoic Nit | !SIO2_ICP on stoic Nit | ||
!SIO2_ICP on low-stress Nit | !SIO2_ICP on low-stress Nit | ||
|- | |- | ||
|Etch rate | |Etch rate | ||
| | |121 nm/min | ||
( | (18.07.2023 mfarin @ DTU nanolab) | ||
|194 nm/min | |194 nm/min | ||
( | (24.05.2023 mfarin @ DTU nanolab) | ||
|190 nm/min | |190 nm/min | ||
( | (24.05.2023 mfarin @ DTU nanolab) | ||
|- | |- | ||
|} | |} | ||
====Results | ====Results with a ''patterned wafer'' ==== | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
Line 90: | Line 62: | ||
|155 nm/min in the center, 125nm/min in the edges | |155 nm/min in the center, 125nm/min in the edges | ||
(03052023 mfarin @ DTU nanolab) | (03052023 mfarin @ DTU nanolab) | ||
| | | | ||
| | |||
| | |||
| | | | ||
|- | |- |
Latest revision as of 15:25, 18 July 2023
Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results with a non-patterned wafer
Recipe | Recipe: SIO2_ICP | SIO2_ICP on stoic Nit | SIO2_ICP on low-stress Nit |
---|---|---|---|
Etch rate | 121 nm/min
(18.07.2023 mfarin @ DTU nanolab) |
194 nm/min
(24.05.2023 mfarin @ DTU nanolab) |
190 nm/min
(24.05.2023 mfarin @ DTU nanolab) |
Results with a patterned wafer