Specific Process Knowledge/Thin film deposition/Deposition of Silver/Deposition of Silver: Difference between revisions
No edit summary |
|||
(10 intermediate revisions by 3 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silver/Deposition_of_Silver click here]''' | |||
''All contents by '''Nanolab staff.''''' | |||
== Thermal deposition of Silver == | == Thermal deposition of Silver == | ||
Silver can be thermally evaporated in Wordentec. | Silver can be thermally evaporated in the [[Specific Process Knowledge/Thin_film_deposition/Wordentec|Wordentec]] and the [[Specific Process Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]]. The process in the Thermal Evaporator (Lesker) is described [[Specific Process Knowledge/Thin_film_deposition/Deposition_of_Silver/Deposition_of_Silver_in_Thermal_Evaporator|here]]. | ||
===Using the Wordentec=== | |||
== Additional information - process parameters that NOT need to be changed == | The Wordentec is useful if you need to deposit a thin layer on more than three wafers: You can load up to six 6" wafers at a time, but you can only add 8 pellets at a time, which in the Wordentec gives a total of approx. 160 nm (or 20 nm per wafer on six wafers). The uniformity for a 6" wafer will also be better in the Wordentec, while in the Thermal Evaporator it is easier to deposit thicker layers. Note that the pumping time for the Wordentec is at least 1 hour, which means that this is much slower than the Thermal Evaporator unless you are depositing thin layers on many wafers. | ||
Use '''process number 22''' in the process list. | |||
Only the thickness needs to be changed. The deposition '''rate is set to 2.5 Å/s''' (contact responsible Nanolab personnel if you like to run with a different rate). | |||
== Additional information - process parameters that do NOT need to be changed == | |||
Here below are the process parameters of the Ag program | Here below are the process parameters of the Ag program in Wordentec. These are already in the program and do not need to be changed- this is written as a back-up to have a list with all process parameters. | ||
Line 29: | Line 40: | ||
'''Master Tooling''' should be set to: 120% (to get the requested layer thickness on the wafer). (Master tooling for Al = 167%). | '''Master Tooling''' should be set to: 120% (to get the requested layer thickness on the wafer). (Master tooling for Al = 167%). | ||
Latest revision as of 12:57, 13 June 2023
Feedback to this page: click here
All contents by Nanolab staff.
Thermal deposition of Silver
Silver can be thermally evaporated in the Wordentec and the Thermal Evaporator. The process in the Thermal Evaporator (Lesker) is described here.
Using the Wordentec
The Wordentec is useful if you need to deposit a thin layer on more than three wafers: You can load up to six 6" wafers at a time, but you can only add 8 pellets at a time, which in the Wordentec gives a total of approx. 160 nm (or 20 nm per wafer on six wafers). The uniformity for a 6" wafer will also be better in the Wordentec, while in the Thermal Evaporator it is easier to deposit thicker layers. Note that the pumping time for the Wordentec is at least 1 hour, which means that this is much slower than the Thermal Evaporator unless you are depositing thin layers on many wafers.
Use process number 22 in the process list.
Only the thickness needs to be changed. The deposition rate is set to 2.5 Å/s (contact responsible Nanolab personnel if you like to run with a different rate).
Additional information - process parameters that do NOT need to be changed
Here below are the process parameters of the Ag program in Wordentec. These are already in the program and do not need to be changed- this is written as a back-up to have a list with all process parameters.
(These parameters are listed in material 13 Ag the material section: - please contact the process specialist if you are not familiar with this.) For thermal Ag deposition use:
Max power: 6.7 % (With a higher max power, the deposition rate will have large fluctuations).
Soak power 1: 4 %
Soak power 2: 6.6 %
Soak time 2: 1 min
This gives a depositon rate of about 2.5 Å/s (to be set in the process parameters).
To get the right thickness measurement of the quartz crystals, use the prameters
Density: 10.5 (thermal evap. of Al 2.7)
Z-ratio: 0.529 (thermal evap. of Al 1.08)
Master Tooling should be set to: 120% (to get the requested layer thickness on the wafer). (Master tooling for Al = 167%).