'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/AOE_(Advanced_Oxide_Etch)/Silicon_Nitride_Etch_using_AOE/Nitride_etch_with_DUV_mask click here]''' | ||
<br> {{CC-bghe1}} | |||
==Silicon nitride etch - fast - with resist mask== | |||
<gallery caption="Profiles of etched lines. DUV resist mask and about 320nm Si3N4 on Silicon. The barc layer was etch in 1min 15sek with the AOE barcetch recipe, done Marts 2016 by bghe@nanolab " widths="300px" heights="250px" perrow="5"> | |||
Image:duv_sin_03_04.jpg|2min etch: All resist is gone, only a little Si3N4 is left and etched down into the Si | |||
Image:duv_sin_04_06.jpg|30sec etch | |||
Image:duv_sin_04_p1my_13.jpg|30 sec etch - 1µm pitch | |||
Image:duv_sin_04_p3my_07.jpg|30 sec etch - 3µm pitch | |||
Image:duv_sin_04_p3my_10.jpg|30 sec etch - 3 µm pitch | |||
</gallery> | |||
==Silicon nitride etch with the standard silicon oxide etch== | ==Silicon nitride etch with the standard silicon oxide etch== | ||
<gallery caption="Etch of LPCVD nitride with DUV KRF resist as mask. The mask is still on. Made by | <gallery caption="Etch of LPCVD nitride with DUV KRF resist as mask. The mask is still on. Made by bghe@nanolab February 2015 " widths="300px" heights="250px" perrow="3"> | ||
image:DUV_sin_01_2min17.jpg|Profile of lines with 1µm pitch | image:DUV_sin_01_2min17.jpg|Profile of lines with 1µm pitch | ||
image:DUV_sin_01_2min19.jpg|Profile of lines with 4µm pitch | image:DUV_sin_01_2min19.jpg|Profile of lines with 4µm pitch | ||
image:DUV_sin_01_2min20.jpg|Profile of 2µm line - zoom in on 4µm pitch | image:DUV_sin_01_2min20.jpg|Profile of 2µm line - zoom in on 4µm pitch | ||
</gallery> | </gallery> |
Latest revision as of 12:01, 3 February 2023
Feedback to this page: click here
This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated
Silicon nitride etch - fast - with resist mask
-
2min etch: All resist is gone, only a little Si3N4 is left and etched down into the Si
-
30sec etch
-
30 sec etch - 1µm pitch
-
30 sec etch - 3µm pitch
-
30 sec etch - 3 µm pitch
Silicon nitride etch with the standard silicon oxide etch
-
Profile of lines with 1µm pitch
-
Profile of lines with 4µm pitch
-
Profile of 2µm line - zoom in on 4µm pitch