Comparing silicon nitride etch methods at Danchip
Line 118: | Line 118: | ||
![[Specific Process Knowledge/Etch/RIE (Reactive Ion Etch)|RIE (Reactive Ion Etch)]] | ![[Specific Process Knowledge/Etch/RIE (Reactive Ion Etch)|RIE (Reactive Ion Etch)]] | ||
![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]] | ![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]] | ||
![[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/IBSD Ionfab 300]] | ![[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/IBSD Ionfab 300]] | ||
Line 137: | Line 135: | ||
| | | | ||
*AOE | *AOE | ||
| | | | ||
*Primarily for pure physical etch by sputtering with Ar-ions | *Primarily for pure physical etch by sputtering with Ar-ions | ||
Line 168: | Line 162: | ||
*Silicon Nitride | *Silicon Nitride | ||
*Aluminium oxide | *Aluminium oxide | ||
| | | | ||
*Any material that is accepted in the machine | *Any material that is accepted in the machine | ||
Line 198: | Line 178: | ||
| | | | ||
AOE | AOE | ||
| | | | ||
*Process dependant. Has not been tested yet. | *Process dependant. Has not been tested yet. | ||
Line 221: | Line 197: | ||
*<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer | *<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer | ||
*<nowiki>#</nowiki>1 100 mm wafer | *<nowiki>#</nowiki>1 100 mm wafer | ||
*<nowiki>#</nowiki>1 150 mm wafers (only when the system is set up to 150mm) | *<nowiki>#</nowiki>1 150 mm wafers (only when the system is set up to 150mm) | ||
| | | | ||
*As many samples as can be securely fitted on a up to 200mm wafer | *As many samples as can be securely fitted on a up to 200mm wafer | ||
Line 271: | Line 237: | ||
*Aluminium | *Aluminium | ||
*Chromium (try to avoid it) | *Chromium (try to avoid it) | ||
*Quartz/fused silica | *Quartz/fused silica | ||
| | | |
Revision as of 16:04, 11 April 2013
Silicon nitride can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the nitride on the surface (backside and frontside) of a wafer. Dry etching etches one side at a time and can be used to etch structures with several masking materials.
- Wet Silicon Nitride Etch
- Etch of Silicon Nitride using RIE
- Etch of Silicon Nitride using AOE
- IBE/Ion Beam Etching using IBSD Ionfab 300
Comparison of wet Silicon Nitride etch and RIE etch for etching of Silicon Nitride
Wet Silicon Nitride etch | Buffered HF (BHF) | RIE | |
---|---|---|---|
General description |
|
|
|
Possible masking materials |
|
|
|
Etch rate |
|
|
|
Batch size |
|
|
|
Size of substrate |
|
|
|
Allowed materials |
|
|
|
This Part is under construction
Feedback to this page: click here
Comparing silicon nitride etch methods at Danchip ![Section under construction.jpg](/images/thumb/9/9a/Section_under_construction.jpg/70px-Section_under_construction.jpg)
There are a broad varity of silicon nitride etch methods at Danchip. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.
- Wet Silicon Nitride Etch
- Etch of Silicon Nitride using RIE
- Etch of Silicon Nitride using AOE
- IBE/Ion Beam Etching using IBSD Ionfab 300
Compare the methodes for Silicon Nitride etching
Wet Silicon Nitride Etch | BHF | RIE (Reactive Ion Etch) | AOE (Advanced Oxide Etch) | IBE/IBSD Ionfab 300 | |
---|---|---|---|---|---|
Generel description |
|
|
|
|
|
Possible masking materials |
|
|
|
AOE
|
|
Etch rate range |
|
|
|
AOE |
|
Substrate size |
|
|
|
|
|
Allowed materials |
|
|
|
|
|