Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2/Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2/RIE1 Travka results: Difference between revisions
Line 26: | Line 26: | ||
==Process flow and parameters== | ==Process flow and parameters== | ||
{| border="2" cellspacing="0" cellpadding=" | {| border="2" cellspacing="0" cellpadding="3" | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="2"|Photolithography | ||
|style="background:LightGrey; color:black"|Resist thickness | |style="background:LightGrey; color:black"|Resist thickness | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Line 43: | Line 43: | ||
*"Travka80", etch load 80% | *"Travka80", etch load 80% | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="1"|Measure resist thickness | ||
|style="background:LightGrey; color:black"|Filmtek parameters | |style="background:LightGrey; color:black"|Filmtek parameters | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Line 49: | Line 49: | ||
*Points: (x,y) = (10,10);(-10,-10) | *Points: (x,y) = (10,10);(-10,-10) | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="2"|RIE preconditioning | ||
|style="background:LightGrey; color:black"|Before preconditioning | |style="background:LightGrey; color:black"|Before preconditioning | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Line 60: | Line 60: | ||
*Time: 8 minutes | *Time: 8 minutes | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="3"|RIE etching | ||
|style="background:LightGrey; color:black"|Before etching | |style="background:LightGrey; color:black"|Before etching | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Remove native oxide in BHF | ||
|- | |- | ||
|style="background:LightGrey; color:black"|RIE1 etching parameters | |style="background:LightGrey; color:black"|RIE1 etching parameters | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Recipe: "RIETrav2 (same settings as the "OH_polyA" recipe) | ||
*Time: 8 minutes | *Time: 8 minutes | ||
|- | |- | ||
Line 74: | Line 74: | ||
*Etch all wafers the same day | *Etch all wafers the same day | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="1"|Measure resist thickness | ||
|style="background:LightGrey; color:black"|Filmtek parameters | |style="background:LightGrey; color:black"|Filmtek parameters | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Line 80: | Line 80: | ||
*Points: (x,y) = (10,10);(-10,-10) | *Points: (x,y) = (10,10);(-10,-10) | ||
|- | |- | ||
!style="background:silver; color:black" align="left | !style="background:silver; color:black" align="left" rowspan="3"|SEM characterization | ||
|style="background:LightGrey; color:black"|Note | |style="background:LightGrey; color:black"|Note | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Line 101: | Line 101: | ||
|- | |- | ||
|} | |} | ||
==Results== | ==Results== |
Revision as of 11:54, 3 April 2013
THIS PAGE IS UNDER CONSTRUCTION![Under construction.png](/images/thumb/f/f8/Under_construction.png/200px-Under_construction.png.jpeg)
RIE1 Travka results - Silicon etch rate and profile as function of etch load
Purpose
The purpose of the RIE1 Travka experiments is the measure the silicon etch rate and profile as function fo the etch load, i.e. the percentage of the wafer that is etched.
Experiment
Seven silicon wafers have been etched in RIE1 using the "OH_polyA" recipe.
All wafers have the same resist pattern ("Travka" masks), but the etch load is differs from wafer to wafer. A description of the process flow is show below. For more information about the "Travka" masks see Travka masks.
The wafers have been etched in June 2012.
Measurements
After the etching the wafers have been cleaved, and trechnes with different mask widths have been inspected with SEM in order to measure resist etch rate, the Si etch depth, the under etch and the trench width. From the Si etch depth the Si etch rate has been calculated.
The resist thickness has been measured on the Filmtek before and after the RIE etching, and thus the resist etch rate is calculted.
The results of the RIE etching, including SEM images of the etching profiles, are show below.
Process flow and parameters
Photolithography | Resist thickness |
|
---|---|---|
Resist masks and etch loads |
| |
Measure resist thickness | Filmtek parameters |
|
RIE preconditioning | Before preconditioning |
|
RIE1 preconditioning parameters |
| |
RIE etching | Before etching |
|
RIE1 etching parameters |
| |
Note |
| |
Measure resist thickness | Filmtek parameters |
|
SEM characterization | Note |
|
Mask trench widths to be measured |
| |
Measurements |
|
Results
Silicon etch rate as function
- Result of InP etching. David Larsson, DTU Photonics, 2011
A table with the etching result can be found here:
xxx
Mask | Resist etch rate [nm/min] | Silicon etch rate [µm/min] | Trench width [µm] | Under etch [µm] | Silicon etch angle [oC] | ||||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
2 µm | 4 µm | 10 µm | 50 µm | 200 µm | 2 µm | 4 µm | 10 µm | 50 µm | 200 µm | 2 µm | 4 µm | 10 µm | 50 µm | 200 µm | 2 µm | 4 µm | 10 µm | 50 µm | 200 µm | ||||
Travka5 | 67.31 | 0.6 | 0.63 | 0.63 | 0.62 | 0.61 | 2.60 | 4,91 | 10.96 | 51.00 | 201.90 | ||||||||||||
Travka10 | 63.94 | 0.57 | 0.59 | 0.59 | 0.58 | 0.61 | 2.32 | 4.60 | |||||||||||||||
Travka20 | 63.13 | 0.63 | 0.63 | 0.64 | 0.64 | 0.59 | |||||||||||||||||
Travka35 | 59.63 | 0.57 | 0.60 | 0.61 | 0.61 | 0.55 | |||||||||||||||||
Travka50 | 57.13 | 0.47 | 0.5 | 0.51 | 0.51 | 0.49 | |||||||||||||||||
Travka65 | 57.88 | 0.41 | 0.41 | 0.42 | 0.42 | 0.43 | |||||||||||||||||
Travka80 | 57.56 | 0.37 | 0.36 | 0.37 | 0.37 | 0.38 | |||||||||||||||||
Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers |