Specific Process Knowledge/Etch/Etching of Aluminium: Difference between revisions
Jump to navigation
Jump to search
Line 65: | Line 65: | ||
!Substrate size | !Substrate size | ||
| | | | ||
*<nowiki>#</nowiki> | *<nowiki>#</nowiki>1-25 100 mm wafers | ||
| | | | ||
*<nowiki>#</nowiki> | *<nowiki>#</nowiki>1-25 100 mm wafers | ||
*<nowiki>#</nowiki> | | | ||
*<nowiki>#</nowiki> | *smaller pieces on a carrier wafer | ||
*<nowiki>#</nowiki> | *<nowiki>#</nowiki>1 100mm wafers (when set up to 100mm wafers) | ||
*<nowiki>#</nowiki>1 150mm wafers (when set up to 150mm wafers) | |||
| | |||
Smaller pieces glued to carrier wafer | |||
*<nowiki>#</nowiki>1 50mm wafer | |||
*<nowiki>#</nowiki>1 100mm wafer | |||
*<nowiki>#</nowiki>1 150mm wafer | |||
*<nowiki>#</nowiki>1 200mm wafer | |||
|- | |- | ||
Revision as of 13:44, 12 March 2013
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
Etching of Aluminium
Etching of aluminium can be done either by wet etch, dry etch or by sputtering with ions.
Comparison methode 1 and methode 2 for the process
Al wet etch 1 | Al wet etch 2 | Al etch by ICP metal | Al sputtering by IBE (Ionfab300+) | |
---|---|---|---|---|
Generel description | Wet etch of pure Al | Wet etch of Al + 1.5% Si | Dry plasma etch of Al | Sputtering of Al - pure physical etch |
Etch rate range |
|
|
|
|
Etch profile |
|
|
|
|
Substrate size |
|
|
|
Smaller pieces glued to carrier wafer
|
Allowed materials |
|
|