== Process A == | |||
Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load. | |||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
|+ '''Process A specifications''' | |+ '''Process A specifications''' |
Revision as of 12:59, 26 November 2012
Process A
Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.
Parameter | Specification | Average result |
---|---|---|
Etch rate (µm/min) | > 15 | 18.9 |
Etched depth (µm) | 150 | 189.1 |
Scallop size (nm) | < 800 | 718 |
Profile (degs) | 91 +/- 1 | 91.1 |
Selectivity to AZ photoresist | > 150 | 310 |
Undercut (µm) | <1.5 | 0.84 |
Uniformity (%) | < 3.5 | 3.0 |
Repeatability (%) | <4 | 0.43 |
Step 1 | Step 2 | |||
---|---|---|---|---|
Parameter | Etch | Dep | Etch | Dep |
Gas flow (sccm) | SF6 350 (1.5 s) 550 | C4F8 200 | SF6 350 (1.5 s) 550 | C4F8 200 |
Cycle time (secs) | 7.0 | 4.0 | 7.0 | 4.0 |
Pressure (mtorr) | 25 (1.5 s) 90 >> 150 | 25 | 25 (1.5 s) 150 | 25 |
Coil power (W) | 2800 | 2000 | 2800 | 2000 |
Platen power (W) | 120 >> 140 (1.5) 45 | 0 | 140 (1.5) 45 | 0 |
Cycles | 11 (keep fixed) | 44 (vary this) | ||
Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers |