Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec: Difference between revisions

From LabAdviser
Kn (talk | contribs)
New page: == Silicon sputter== Silicon can be deposited in Wordentec. '''Parameters''' Listed below are tried parameters, that can ...
 
Kn (talk | contribs)
No edit summary
Line 8: Line 8:
Listed below are tried parameters, that can be used during deposition.
Listed below are tried parameters, that can be used during deposition.


Please don´t use higher power then 180W, since the target then could breake into a lot of small pieces.


{| border="1" cellspacing="0" cellpadding="4"  
{| border="1" cellspacing="0" cellpadding="4"  

Revision as of 14:11, 15 August 2012

Silicon sputter

Silicon can be deposited in Wordentec.


Parameters

Listed below are tried parameters, that can be used during deposition.


Please don´t use higher power then 180W, since the target then could breake into a lot of small pieces.

Setting
Process type Sputtering
Power 1000W
Base pressure 6*10-7
Ignition pressure 6*10-3
Sputter pressure 4*10-3
Rate About 0,14Å/s (2 wafers plates, rotating)