Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
Line 71: Line 71:
|-  
|-  
| SF<sub>6</sub> flow
| SF<sub>6</sub> flow
|32 sccm
|30 sccm
|-
|-
|O<sub>2</sub> flow
|O<sub>2</sub> flow
Line 89: Line 89:


Here are a few images of some of the single experiments in the DOE. The width of the trenches are roughly 1.5µm:
Here are a few images of some of the single experiments in the DOE. The width of the trenches are roughly 1.5µm:
{| border="1" cellspacing="1" cellpadding="2"  align="left"
{| border="1" cellspacing="1" cellpadding="2"
!
[[image:DOE RIE1 O2245 CHF310 P36.jpg|100x100px|thumb|center|O2:24.5sccm CHF3:10sccm Pressure:36mTorr]]
!
[[image:DOE RIE1 O229 CHF315 P31.jpg|100x100px|thumb|center|O2:29sccm CHF3:15sccm Pressure:31mTorr]]
!
[[image:DOE RIE1 O220 CHF35 P31.jpg|100x100px|thumb|center|O2:20sccm CHF3:5sccm Pressure:31mTorr
]]
|}
 
 
===RIE2:===
[[image:RIE1_Si_Angle_O2_CHF3.jpg|300x300px|thumb|right|Angle of sidewall on 1.5 µm trenches - independent on pressure within the given pressure range]]
A Design Of Experiment (DOE) has been performed. Here is a short summary:
 
 
 
{| border="1" cellspacing="1" cellpadding="2"  align="center"
! Recipe:
!
|-
| SF<sub>6</sub> flow
|30 sccm
|-
|O<sub>2</sub> flow
|20-29 sccm
|-
|CHF<sub>3</sub> flow
|5-15 scmm
|-
|Pressure
|36 mTorr
|-
|RF-power
|20 W
|-
|}
More details on the DOE can be seen here: "DOE RIE2 silicon etch of small structures".
 
Here are a few images of some of the single experiments in the DOE. The width of the trenches are roughly 1.5µm:
{| border="1" cellspacing="1" cellpadding="2"  
!
!
[[image:DOE RIE1 O2245 CHF310 P36.jpg|100x100px|thumb|center|O2:24.5sccm CHF3:10sccm Pressure:36mTorr]]
[[image:DOE RIE1 O2245 CHF310 P36.jpg|100x100px|thumb|center|O2:24.5sccm CHF3:10sccm Pressure:36mTorr]]

Revision as of 09:32, 13 November 2007

RIE (Reactive Ion Etch) can be used for etching silicon - both crystalline and polycrystalline silicon. The etch can be isotropic or anisotropic with vertical sidewalls depending on the process recipe and the masking material and geometry. The Si is etched by flour radicals that are created from SF6(g) in a RF generated plasma.

The silicon substrate:

Most be a wafer of 4" or below or small pieces, not higher than about 2mm.

The silicon can be masked by these materials:

  • Photoresist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)

Most used recipe (this recipe is being watched in the in the quality assurance program):

Recipe: OH_POLYA
SF6 flow 32 sccm
O2 flow 8 sccm
Pressure 80 mTorr
RF-power 30 W
Expected results in RIE1 Expected results in RIE2
Etch rate in Si ~0.40 µm/min ~0.45 µm/min
Etch rate in Si3N4 ~0.05 µm/min
Etch rate in SiO2 ~0.02 µm/min


The etching results are dependent on the mask geometry primarily the etch load (meaning the area fraction of the silicon substrate that is exposed to the plasma). To illustrate that you can see on the images below the effect of mask load on the results of the OH_PolyA recipe. The first one has a load of 10-20% and the second has a load of 50%. It can be seen that the sidewalls are closer to vertical with 50% load than with 10 % load. Also the etch rate is effected by the load.

RIE1: OH_Polya on load ~10% 4 min. Etch rate:~0.47 µm/min
RIE1: OH_Polya on load 50% 4 min. Etch rate:~0.61µm/min

Etch of small structures

RIE1:

Angle of sidewall on 1.5 µm trenches - independent on pressure within the given pressure range

A Design Of Experiment (DOE) has been performed. Here is a short summary:


Recipe:
SF6 flow 30 sccm
O2 flow 20-29 sccm
CHF3 flow 5-15 scmm
Pressure 31-41 mTorr
RF-power 20 W

More details on the DOE can be seen here: "DOE RIE1 silicon etch of small structures".

Here are a few images of some of the single experiments in the DOE. The width of the trenches are roughly 1.5µm:

O2:24.5sccm CHF3:10sccm Pressure:36mTorr
O2:29sccm CHF3:15sccm Pressure:31mTorr
O2:20sccm CHF3:5sccm Pressure:31mTorr


RIE2:

Angle of sidewall on 1.5 µm trenches - independent on pressure within the given pressure range

A Design Of Experiment (DOE) has been performed. Here is a short summary:


Recipe:
SF6 flow 30 sccm
O2 flow 20-29 sccm
CHF3 flow 5-15 scmm
Pressure 36 mTorr
RF-power 20 W

More details on the DOE can be seen here: "DOE RIE2 silicon etch of small structures".

Here are a few images of some of the single experiments in the DOE. The width of the trenches are roughly 1.5µm:

O2:24.5sccm CHF3:10sccm Pressure:36mTorr
O2:29sccm CHF3:15sccm Pressure:31mTorr
O2:20sccm CHF3:5sccm Pressure:31mTorr