[[Image:fumehoodetch-chrom.jpg|300x300px|thumb|Fume hood: positioned in cleanroom 2. <br />Wet Etch of Chromium can take place in a beaker in this fume hood]] | [[Image:fumehoodetch-chrom.jpg|300x300px|thumb|Fume hood: positioned in cleanroom 2. <br />Wet Etch of Chromium can take place in a beaker in this fume hood]] | ||
Wet etching of chromium at Danchip is done making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this: | |||
# HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g - standard at Danchip | # HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g - standard at Danchip | ||
Line 73: | Line 73: | ||
|- | |- | ||
|} | |} | ||
== Dry etching of chromium == | |||
On the [[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch]] tool a recipe for chromium is being developed. |
Revision as of 14:05, 11 July 2011
Wet etching of Chromium
Wet etching of chromium at Danchip is done making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:
- HNO:HO:cerisulphate - 90ml:1200ml:15g - standard at Danchip
- Commercial chromium etch
Etch rate are depending on the level of oxidation of the metal.
How to mix the Chromium etch 1:
- Take a beaker and add 15g of cerisulphate.
- Add a little water while stirring - make sure all lumps are gone.
- Add water until 600 ml - keep stirring (use magnetic stirring)
- Add 90 ml HNO
- When the cerisulphate is completely dissolved (clear liquid) you can add the other 600 ml of wafer.
Overview of the data for the chromium etches
Chromium etch 1 | Chromium etch 2 | |
---|---|---|
General description |
Etch of chromium |
Etch of chromium |
Chemical solution | HNO:HO:cerisulphate - 90ml:1200ml:15g | . |
Process temperature | Room temperature | . |
Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
. |
Etch rate |
~40-100 nm/min |
. |
Batch size |
1-25 wafers at a time |
. |
Size of substrate |
4" wafers |
. |
Allowed materials |
No restrictions. Make a note on the bottle of which materials have been processed. |
. |
Dry etching of chromium
On the ICP Metal Etch tool a recipe for chromium is being developed.