Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride: Difference between revisions
No edit summary |
mNo edit summary |
||
(4 intermediate revisions by 3 users not shown) | |||
Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride&action=submit click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride&action=submit click here]''' | ||
== Deposition of silicon nitride == | == Deposition of silicon nitride == | ||
Deposition of silicon nitride can be done | Deposition of silicon nitride can be done by either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stoichiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace. PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a much lower temperature and a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well. | ||
It is also possible to deposit silicon nitride | It is also possible to deposit silicon nitride and oxynitride by reactive sputtering. | ||
*[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace|Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace]] | *[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace|Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace]] | ||
Line 14: | Line 17: | ||
*[[/Deposition of silicon nitride using Lesker sputter system|Nitride deposition using Lesker sputter system]] | *[[/Deposition of silicon nitride using Lesker sputter system|Nitride deposition using Lesker sputter system]] | ||
==Comparison of LPCVD, PECVD and | *[[/Deposition of silicon nitride using Sputter-System Metal-Oxide(PC1)|Nitride deposition using Sputter-System Metal-Oxide(PC1)]] | ||
==Comparison of LPCVD, PECVD, and sputter systems for silicon nitride deposition== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
Line 24: | Line 29: | ||
![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|LPCVD]] | ![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|LPCVD]] | ||
![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ||
![[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Nitride(PC3) and Sputter-System Metal-Oxide(PC1)]] | |||
![[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputter system]] | ![[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputter system]] | ||
|- | |- | ||
Line 30: | Line 36: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | | | ||
|Plasma Enhanced Chemical Vapour Deposition (PECVD process) | *Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | ||
|Reactive sputtering | | | ||
*Plasma Enhanced Chemical Vapour Deposition (PECVD process) | |||
| | |||
*Reactive sputtering | |||
*Pulsed DC reactive sputtering | |||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | |||
|*Reactive sputtering | |||
|- | |- | ||
Line 45: | Line 57: | ||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | *Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | ||
Silicon nitride can be doped with boron or phosphorus | Silicon nitride can be doped with boron or phosphorus | ||
|Unknown | | | ||
*Si<sub>x</sub>N<sub>y</sub> (Sputter-System Metal-Nitride(PC3)) | |||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub> (Sputter-System Metal-Oxide(PC1)) | |||
Tunable composition | |||
| | |||
*Unknown | |||
|- | |- | ||
Line 57: | Line 74: | ||
| | | | ||
*~40 nm - 10 µm | *~40 nm - 10 µm | ||
|limited by process time. | | | ||
Deposition rate | *limited by process time. | ||
*Deposition rate likely faster than Sputter-System (Lesker) | |||
| | |||
*limited by process time. | |||
*Deposition rate ~ 1-5 nm/min | |||
|- | |- | ||
Line 65: | Line 87: | ||
!Process temperature | !Process temperature | ||
| | | | ||
*Stoichiometric nitride: 780 | *Stoichiometric nitride: 780 °C - 800 °C | ||
*Silicon rich (low stress) nitride: 810 | *Silicon rich (low stress) nitride: 810 °C - 845 °C | ||
| | |||
*300 °C | |||
| | |||
*Up to 600 °C | |||
| | | | ||
* | *Up to 400 °C | ||
|- | |- | ||
Line 79: | Line 104: | ||
| | | | ||
*Less good | *Less good | ||
| | | | ||
*some step coverage possible, especially by HIPIMS | |||
| | |||
*some step coverage possible but amount unknown | |||
|- | |- | ||
Line 93: | Line 121: | ||
*Less dense film | *Less dense film | ||
*Incorporation of hydrogen in the film | *Incorporation of hydrogen in the film | ||
| | |||
*Deposition on one side of the substrate | |||
*Less dense film | |||
*Properties including density tunable (requires process development) | |||
| | | | ||
*Deposition on one side of the substrate | *Deposition on one side of the substrate | ||
*unknown quality | *unknown quality | ||
*likely O-contamination | |||
|- | |- | ||
Line 105: | Line 138: | ||
| | | | ||
*Dependent on recipe: ~1-10 Å/min | *Dependent on recipe: ~1-10 Å/min | ||
|Unknown | | | ||
*Unknown | |||
| | |||
*Unknown | |||
|- | |- | ||
Line 112: | Line 148: | ||
!BHF etch rate | !BHF etch rate | ||
| | | | ||
*Very low | *Very low ([[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride|more info here]]) | ||
| | |||
*Very high compared the LPCVD nitride ([[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride|more info here]]) | |||
| | |||
*Unknown | |||
| | | | ||
* | *Unknown | ||
|- | |- | ||
Line 130: | Line 169: | ||
*1 150 mm wafer | *1 150 mm wafer | ||
Depending on what PECVD you use | Depending on what PECVD you use | ||
| | |||
*many smaller samples | |||
*Up to 10*100 mm or 150 mm wafers | |||
| | | | ||
*Several smaller samples | *Several smaller samples | ||
Line 153: | Line 195: | ||
*III-V materials (in PECVD4) | *III-V materials (in PECVD4) | ||
*Small amount of metals (in PECVD3) | *Small amount of metals (in PECVD3) | ||
|Any | | | ||
*Almost any as long as they do not outgas and are not very toxic, see cross-contamination sheets | |||
| | |||
*Any | |||
|- | |- | ||
|} | |} |
Latest revision as of 14:58, 6 March 2025
The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.
Feedback to this page: click here
Deposition of silicon nitride
Deposition of silicon nitride can be done by either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stoichiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace. PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a much lower temperature and a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well.
It is also possible to deposit silicon nitride and oxynitride by reactive sputtering.
- Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace
- Deposition of silicon rich (low stress) nitride using the 6" LPCVD nitride furnace
- Nitride deposition using PECVD (or oxynitride)
Comparison of LPCVD, PECVD, and sputter systems for silicon nitride deposition
LPCVD | PECVD | Sputter-System Metal-Nitride(PC3) and Sputter-System Metal-Oxide(PC1) | Lesker sputter system | |
---|---|---|---|---|
Generel description |
|
|
|
*Reactive sputtering |
Stoichiometry |
|
Silicon nitride can be doped with boron or phosphorus |
Tunable composition |
|
Film thickness |
Thicker nitride layers can be deposited over more runs (maximum two) |
|
|
|
Process temperature |
|
|
|
|
Step coverage |
|
|
|
|
Film quality |
|
|
|
|
KOH etch rate (80 oC) |
|
|
|
|
BHF etch rate |
|
|
|
|
Batch size |
|
Depending on what PECVD you use |
|
|
Allowed materials |
Processed wafers have to be RCA cleaned |
|
|
|