Specific Process Knowledge/Lithography/CSAR: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
Thope (talk | contribs)
 
(343 intermediate revisions by 4 users not shown)
Line 1: Line 1:
These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.




== Process Flow ==
Test of Chemically Semi-Amplified Resist (CSAR); a positive e-beam resist from AllResist (AR-P 6200-2).


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;"
|-
|-
|-style="background:Black; color:White"
!Equipment
!Process Parameters
!Comments
|-
|-
|-style="background:WhiteSmoke; color:black; text-align:center"
!colspan="4"|Pretreatment
|-


Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.


|-
|-style="background:LightGrey; color:black"
|4" Si wafers
|No Pretreatment
|
|-


|-
== Spin Curves ==
|-style="background:WhiteSmoke; color:black; text-align:center"
!colspan="4"|Spin Coat
|-




|-
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.  
|-style="background:LightGrey; color:black"
|Spin Coater Manual, LabSpin, A-5
|AR-P 6200/2 AllResist E-beam resist
60 sec at various spin speed.
Acceleration 4000 s-2,
softbake 1 - 5 min at 150 deg Celcius
|Disposal pipette used; clean by N2-gun before use. Use approximately 1.5 ml per 4" wafer, never use a pipette twice. Softbake is not a crucial step, see e-mail correspondence with AllResist [[media:Softbake CSAR.pdf|here]].
|-


|-
Around 2 ml of resist per wafer has been used when fabricating these curves. If you use less than 2 ml, the thickness of the final resist might be smaller than reported here.
|-style="background:WhiteSmoke; color:black; text-align:center"
!colspan="4"|Characterization
|-


|-
|-style="background:LightGrey; color:black"
|Ellipsometer VASE B-1
|9 points measured on 100 mm wafer
|ZEP program used; measured at 70 deg only
|-


|-
[[File:CSAR_09.png|right|600px]]
|-style="background:WhiteSmoke; color:black; text-align:center"
[[File:CSAR_18.png|right|600px]]
!colspan="4"|E-beam Exposure
|-




|-
|-style="background:LightGrey; color:black"
|JEOL 9500 E-beam writer, E-1
|Dosepattern 15nm - 100nm,
dose 120-280 muC/cm2
|Virtual chip mark height detection (CHIPAL V1) used in corner of every dose array
|-
|-
|-style="background:WhiteSmoke; color:black; text-align:center"
!colspan="4"|Development
|-
|-
|-style="background:LightGrey; color:black"
|Fumehood, D-3
|60 sec in X AR 600-54/6,
60 sec rinse in IPA,
N2 Blow dry
|Gentle agitation while developing. After developing, wafer is immersed in beaker with IPA, subsequently blow dried with N2 gun.
|-
|-
|-style="background:WhiteSmoke; color:black; text-align:center"
!colspan="4"|Characterization
|-
|-
|-style="background:LightGrey; color:black"
|Zeiss SEM Supra 60VP, D-3
|2 kV, shortest working distance possible, chip mounted with Al tape
|The wafers are diced into smaller pieces and sputter coated with Pt at DTU CEN before SEM inspection; please contact [mailto:ramona.mateiu@cen.dtu.dk|Ramona Valentina Mateiu] for further information.
|-
|}
== Spin Curves ==
[[File:SpinCurveCSAR.jpg|right|600px]]
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 40%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 40%"
Line 109: Line 23:


|-
|-
|-style="background:Black; color:White"
|-style="background:#00308F; color:White"
!colspan="7"|AllResist AR-P 6200/2 spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
!colspan="7"|AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
|-
|-


Line 118: Line 32:
!Acceleration [1/s2]
!Acceleration [1/s2]
!Thickness [nm]
!Thickness [nm]
!St Dev
|-
|-


Line 125: Line 38:
|2000
|2000
|4000
|4000
|225.98
|226
|0.97
|-
|-


Line 133: Line 45:
|3000
|3000
|4000
|4000
|194.00
|194
|0.6
|-
|-


Line 141: Line 52:
|4000
|4000
|4000
|4000
|169.57
|170
|0.32
|-
|-


Line 149: Line 59:
|5000
|5000
|4000
|4000
|151.47
|151
|0.26
|-
|-


Line 157: Line 66:
|6000
|6000
|4000
|4000
|142.38
|142
|0.41
|-
|-


Line 165: Line 73:
|7000
|7000
|4000
|4000
|126.59
|127
|0.36
|-
|-


Line 177: Line 84:


|-
|-
|-style="background:green; color:White"
|-style="background:red; color:White"
!colspan="7"|AllResist CSAR on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
!colspan="7"|AllResist CSAR 6200.09 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
|-
|-


Line 186: Line 93:
!Acceleration [1/s2]
!Acceleration [1/s2]
!Thickness [nm]
!Thickness [nm]
!St Dev
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2000
|4000
|84
|-
|-


Line 193: Line 106:
|3000
|3000
|4000
|4000
|201.61
|67
|1.20
|-
|-


Line 201: Line 113:
|4000
|4000
|4000
|4000
|173.89
|59
|0.64
|-
|-


Line 209: Line 120:
|5000
|5000
|4000
|4000
|155.91
|53
|0.65
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|6000
|4000
|49
|-
|-


Line 221: Line 138:


|-
|-
|-style="background:red; color:White"
|-style="background:green; color:White"
!colspan="7"|AllResist CSAR 1:1 in anisole, Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
!colspan="7"|AllResist CSAR 6200.18 (< 2ml per 4" wafer), Spin Coater: Manual Standard Resists, E-5, TIGRE, 15-06-2016. Softbake 2 min @ 180 degC.
|-
|-


Line 230: Line 147:
!Acceleration [1/s2]
!Acceleration [1/s2]
!Thickness [nm]
!Thickness [nm]
!St Dev
|-
|-


Line 236: Line 152:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|2000
|2000
|4000
|2000
|83.48
|1003
|0.49
|-
|-


Line 244: Line 159:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|3000
|3000
|4000
|2000
|67.12
|809
|0.41
|-
|-


Line 252: Line 166:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|4000
|4000
|4000
|2000
|58.64
|721
|0.44
|-
|-


Line 260: Line 173:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|5000
|5000
|4000
|2000
|53.13
|639
|0.39
|-
|-


Line 268: Line 180:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|6000
|6000
|4000
|2000
|48.76
|586
|0.38
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|7000
|2000
|549
|-
|-


|}
|}


<br>
<br>
<br>
== Contrast Curve ==


== SEM pictures of dosepatterns ==
=== CSAR 6200.09 ===


=== 53 nm CSAR ===
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;"
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%"
|-
|-


|-
|-
|-style="background:Black; text-align:left; color:White"
|-style="background:Black; color:White"
!Process
!colspan="5"|CSAR Contrast Curve, Processed by TIGRE, FEB-MARCH 2016
!Equipment
!Parameters
!Date and initials
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|Resist
!Resist
|Fumehood D-3
!Spin Coat
|AR-P 6200/2 AllResist E-beam resist diluted 1:1 in anisole
!E-beam exposure
|16-06-2014 TIGRE
!Development
!Characterisation
|-
|-


|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|Spin Coat
|CSAR AR-P6200.09 AllResist, CSAR AR-P6200.09 diluted 1:1 in Anisole
|Spin Coater LabSpin A-5
|08-02-2016, LabSpin E-5, 4000 rpm, 60s, softbaked 60s @ 205 degC
|1 min @ 5000 rpm, 4000 1/s2, softbake 2 min @ 150 degC, thickness ~53nm
|09-02-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces
|16-06-2014 TIGRE
|11-02-2016, Fumehood D-2, AR-600-546, rinsed in IPA 60s.
|02-03-2016 AFM Icon, F-2, ScanAsyst in Air
|-
|-


|}
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
|-
|-style="background:WhiteSmoke; color:black"
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]]
|E-beam exposure
|-  
|JEOL 9500 E-2
| colspan="1" style="text-align:center;|
|0.2 nA, aperture 5, dose 207-242 muC/cm2, SHOT A,10
AR-P 6200 contrast curves.
|02-07-2014 TIGRE
|}
 
==Dose to size==
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.
 
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
|-
| [[image:thope240214_lines_100_06.png|1200px]]
|-
| [[image:thope240214_lines_50_11.png|1200px]]
|-
| [[image:thope240214_lines_20_13.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines250_100nm.png|1200px]]
|-
| [[image:thope240214_lines250_50nm.png|1200px]]
|-
| [[image:thope240214_lines250_20nm.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
|-
|-style="background:WhiteSmoke; color:black"
| [[image:thope240214_lines180_100_29.png|1200px]]
|Develop
|-  
|Fumehood D-3
| [[image:thope240214_lines180_50_31.png|1200px]]
|SX-AR 600-54/6 60 sec, 60 sec IPA rinse
|-
|08-07-2014 TIGRE
| [[image:thope240214_lines180_20_33.png|1200px]]
|-  
| colspan="1" style="text-align:center;|
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
 
=== CSAR 6200.18 ===
 
100 nm lines in ~900 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.
 
[[File:CSAR 6200.18 developed with AR600546.png|right|400px]]
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:right;"  style="width: 60%"
|-
|-


|-
|-style="background:Black; color:White"
!colspan="5"|CSAR Contrast Curve, Processed by TIGRE, JUNE 2016
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|Sputter Coat
!Resist
|Cressington 208HR, DTU CEN
!Spin Coat
|3-5 nm Pt, sputtering
!E-beam exposure
|09-07-2014 TIGRE
!Development
!Characterisation
|-
|-


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|Characterization
|CSAR AR-P6200.18 AllResist
|Zeiss SEM Supra 60VP, D-3
|15-06-2016, LabSpin E-5, 2000 rpm, 60s, softbaked 60s @ 205 degC
|3 kV, WD below 4mm, conducting tape close to pattern
|15-06-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces
|09-07-2014, TIGRE
|16-06-2016, Fumehood E-4, AR-600-546, 30s/60s/90s, rinsed in IPA 60s.
|JUNE/JULY 2016 SEM Supra 2, 10 keV
|-
|-


|}
|}


<br clear="all"/>
=== Dark Erosion ===
Dark erosion has been measured on a un-exposed 4" wafer spin coated with CSAR 6200.18 to a thickness of approximately 549 nm. The resist thickness has been measured by VASE Ellipsometer before development, and after 3 minutes, 13 minutes, and 30 minutes of development in AR 600 546.
The graphs shows the measured thicknesses; the errorbars represents the standard deviations from the ellipsometric measurements. The average etch rate of CSAR is ~0.1 nm/min.


'''50nm'''
[[File:dark erosion.png|right|400px]]


{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
! width="100" | dose [muC/cm2]
! width="250" | 207
! width="250" | 219
! width="250" | 230
! width="250" | 242
|-
|
| [[File:CSAR50nmoverview-10%.png|250px]]
| [[File:CSAR50nmoverview-5%.png|250px]]
| [[File:CSAR50nmoverview.png|250px]]
| [[File:CSAR50nmoverview+5%.png|250px]]
|-
|
| [[File:CSAR50nmlines-10%.png|250px]]
| [[File:CSAR50nmlines-5%.png|250px]]
| [[File:CSAR50nmlines.png|250px]]
| [[File:CSAR50nmlines+5%.png|250px]]


|}


<br clear="all" />


'''30nm'''
== Development ==


{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
Many resists can be developed in different developers, CSAR can be developed in: AR 600-546, AR 600-548, ZED N-50 and mix of MIBK and IPA among others.  
! width="100" | dose [muC/cm2]
! width="250" | 207
! width="250" | 219
! width="250" | 230
! width="250" | 242
|-  
|
| [[File:CSAR30nmoverview-10%.png|250px]]
| [[File:CSAR30nmoverview-5%.png|250px]]
| [[File:CSAR30nmoverview.png|250px]]
| [[File:CSAR30nmoverview+5%.png|250px]]
|-  
|
| [[File:CSAR30nmlines-10%.png|250px]]
| [[File:CSAR30nmlines-5%.png|250px]]
| [[File:CSAR30nmlines.png|250px]]
| [[File:CSAR30nmlines+5%.png|250px]]


|}
CSAR and ZEP520A are in principle the same chemical, however the pretreatment (filtration and temperature control) can differ.


Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.


'''20nm'''
When this is said some users still observe residues when using AR 600-546, the producer "'''All resist GMBH'''" have recommended to use 3-5s, dip in pure MIBK to remove residues.
AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds.


{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
<br clear="all"/>
! width="100" | dose [muC/cm2]
! width="250" | 230
! width="250" | 242
! width="250" | 253
|-
|
| [[File:CSAR20nmoverview.png|250px]]
| [[File:CSAR20nmoverview+5%.png|250px]]
| [[File:CSAR20nmoverview+10%.png|250px]]
|-


== Etch Tests ==


|}
If you have wafers or chips with CSAR you would like to have tested, please send me an [[mailto:tigre@danchip.dtu.dk email]].


=== Chlorine versus flourine-based etches ===


We have experienced problems with removal of CSAR after chlorine-based dry etch, see the file [[:File:DryEtchTestsCSAR.pdf]]. It seems the chlorine etch forms particles of chlorinated CSAR on the surface, and these particles remains on the surface after resist removal with AR-600-71. The C4F8/SF6 etch also forms particles on the surface, but much smaller than those formed in the chlorine etch. It seems these particles are removed after 3 minutes in AR-600-71.


=== 140 nm CSAR ===
=== How to mount chips in dry etch tools ===


All etch rates presented here are measured on chips (i.e. diced 4" wafers) crystal bonded to a carrier. The carrier is either a blank Si wafer, a Si wafer spin coated with resist or a Si wafer coated with ALD grown Al2O3.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 60%;"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%;"
|-
|+style="background:Black; color:White"  colspan="4"|'''Etch Tests of CSAR, recipe 'nano1.42', DRIE PEGASUS, A-1. CSAR thickness measured on Ellipsometer VASE at 70 degrees'''
|-
|-
!rowspan="1"|Sample
!colspan="1"|CSAR Etch rate nm/min
|-
|-
 
|Full 4" Si wafer with non-patterned ~180 nm CSAR
|~56.5 (based on 2 runs)
|-
|-
|-style="background:Black; text-align:left; color:White"
!Process
!Equipment
!Parameters
!Date and initials
|-
|-
 
|Full 4" Si wafer with non-patterned ~240 nm CSAR, <br>postbaked 60 sec @ 130 degC
|~56.5 (based on 2 runs)
|-
|-
|-style="background:WhiteSmoke; color:black"
|Resist
|Fumehood D-3
|AR-P 6200/2 AllResist E-beam resist
|2013 (bottle opened)
|-
|-
 
|1/4 4" Si wafer with non-patterned ~125 nm CSAR, <br>not crystal bonded to Si carrier
|-style="background:WhiteSmoke; color:black"
|~83.3 (based on 3 runs)
|Spin Coat
|Spin Coater LabSpin A-5
|1 min @ 6000 rpm, 4000 1/s2, softbake 5 min @ 150 degC, thickness ~143nm
|09-04-2014 TIGRE
|-
|-
|-
|-
|-style="background:WhiteSmoke; color:black"
|1/4 4" Si wafer with non-patterned ~125 CSAR, <br>crystal bonded to 4" Si carrier
|E-beam exposure
|~54 (based on 1 run)
|JEOL 9500 E-2
|2 nA, aperture 5, dose 207-242 muC/cm2, SHOT A,10
|10-04-2014 TIGRE
|-
|-
|}


=== Etch rates and profile inspection ===


==== Continous Etches ====
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 80%;"
|-
|-
|-style="background:WhiteSmoke; color:black"
|+style="background:Black; color:White"  colspan="4"|'''Recipe nano1.42 on Deep Reactive Ion Etch PEGASUS A-1'''
|Develop
|-
|Fumehood D-3
|-
|SX-AR 600-54/6 60 sec, 60 sec IPA rinse
! rowspan="4" align="center"| Recipe
|April/May-2014 TIGRE
| Gasses
| C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<sub>6</sub> 38 sccm
|rowspan="7" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 2:30 minutes (150s) with recipe 'nano1.42'
[[File:617817 HD-4_11.png|200px]] [[File:617817 HD-4_18.png|200px]]
[[File:617817 HD-4_16.png|200px]] [[File:617817 HD-4_14.png|200px]]
|-
|-
| Pressure
| 4 mTorr,
Strike: 3 secs @ 15 mTorr


|-
| Power
| 800 W Coil Power,
40 W Platen Power


|-
|Platen temperature
| - 20°C
|-
|-
|-style="background:WhiteSmoke; color:black"
 
|Sputter Coat
! rowspan="1" align="center"| Conditions
|Cressington 208HR, DTU CEN
| Conditioning
|2-3 nm Pt, sputtering
| Pre-clean: 10 min oxygen clean
|22-05-2014 TIGRE
5 min oxygen clean between runs
|-
|-
 
! rowspan="2" align="center"| Etch rates
 
| Si
|
500 nm lines: ~200 nm/min <br>
190 nm lines: ~200 nm/min <br>
102 nm lines: ~190 nm/min <br>
61 nm lines: ~170 nm/min
|-
|-
|-style="background:WhiteSmoke; color:black"
|CSAR
|Characterization
| ~55 nm/min
|Zeiss SEM Supra 60VP, D-3
|2 kV, WD below 4mm, conducting tape close to pattern
|06-06-2014, TIGRE
|-
|-
|}
|}






'''50nm'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 80%;"
|-
|+style="background:Black; color:White"  colspan="4"|'''Recipe processC on Deep Reactive Ion Etch PEGASUS A-1'''
|-
|-
! rowspan="4" align="center"| Recipe
| Gasses
| C<sub>4</sub>F<sub>8</sub> 70 sccm, SF<sub>6</sub> 38 sccm
|rowspan="7" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 60s with recipe 'ProcessC'
[[File:tigre 6.17 0% 3b_ 07.png|200px]] [[File:tigre 6.17 0% 3b_ 16.png|200px]]
[[File:tigre 6.17 0% 3b_ 14.png|200px]] [[File:tigre 6.17 0% 3b_ 11.png|200px]]
|-
| Pressure
| 4 mTorr,
Strike:  secs @  mTorr


{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
|-
! width="100" | dose [muC/cm2]
| Power
! width="250" | 207
| 450 W Coil Power, 100 W Platen Power
! width="250" | 219
! width="250" | 230
! width="250" | 242
|-  
|-  
|
|Platen temperature
| [[File:CSAR50nmoverview-10%.png|270px]]
| 10°C
| [[File:CSAR50nmoverview-5%.png|270px]]
|-
| [[File:CSAR50nmoverview.png|270px]]
 
| [[File:CSAR50nmoverview+5%.png|270px]]
! rowspan="1" align="center"| Conditions
|-  
| Conditioning
|
| Pre-clean: 10 min oxygen clean
| [[File:CSAR50nmlines-10%.png|270px]]
5 min oxygen clean between runs
| [[File:CSAR50nmlines-5%.png|270px]]
|-
| [[File:CSAR50nmlines.png|270px]]
! rowspan="2" align="center"| Etch rates
| [[File:CSAR50nmlines+5%.png|270px]]
| Si
|  
500 nm lines: ~300 nm/min <br>
102 nm lines: ~250 nm/min <br>


|-
|CSAR
| 158 nm/min
|-
|}
|}


==== Bosch Etch ====


'''30nm'''


{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 80%;"
! width="100" | dose [muC/cm2]
|-
! width="250" | 207
|+style="background:Black; color:White"  colspan="4"|'''Recipe NBoost01 on Deep Reactive Ion Etch PEGASUS A-1'''
! width="250" | 219
|-
! width="250" | 230
|-
! width="250" | 242
! rowspan="13" align="center"  width ="70"| Recipe
|-
| rowspan="4"  width ="50"| Deposition step
|
|Duration
| [[File:CSAR30nmoverview-10%.png|250px]]
| width ="100" |2.5 s
| [[File:CSAR30nmoverview-5%.png|250px]]
|rowspan="16" width="20%" | Profiles of lines exposed at 300 µC/cm2, etched 6:00 minutes with recipe 'NBoost01'
| [[File:CSAR30nmoverview.png|250px]]
[[File:tigre 6.17 -15% 3a_ 11.png|200px]] [[File:tigre 6.17 3a_ 08.png|200px]]
| [[File:CSAR30nmoverview+5%.png|250px]]
[[File:tigre 6.17 3a_ 20.png|200px]] [[File:tigre 6.17 3a_ 21.png|200px]]
|-  
[[File:tigre 6.17 3a_ 22.png|200px]]
|
 
| [[File:CSAR30nmlines-10%.png|250px]]
|-
| [[File:CSAR30nmlines-5%.png|250px]]
| width ="30"| Gasses
| [[File:CSAR30nmlines.png|250px]]
|C<sub>4</sub>F<sub>8</sub> 50 sccm, SF<sub>6</sub> 0 sccm
| [[File:CSAR30nmlines+5%.png|250px]]
|-
| Pressure
|10 mTorr
|-
| Powers
|500 W Coil
|-
| rowspan="4"| Etch step (boost)
|Duration
|1.5 s
|-
| Gasses
|C<sub>4</sub>F<sub>8</sub> 0 sccm, SF<sub>6</sub> 60 sccm
|-
| Pressure
|5 mTorr
|-
| Powers
|400 W Coil, 50 W Platen
|-


|}
| rowspan="4"| Etch step (main)
 
|Duration
 
|3.5 s
'''20nm'''
|-
 
| Gasses
{| cellpadding="2" style="border: 1px solid darkgray;" class="wikitable"
|C<sub>4</sub>F<sub>8</sub> 40 sccm, SF<sub>6</sub> 60 sccm
! width="100" | dose [muC/cm2]
|-
! width="250" | 230
| Pressure
! width="250" | 242
|15 mTorr
! width="250" | 253
|-
|-  
| Powers
|
|400 W Coil, 20 W Platen
| [[File:CSAR20nmoverview.png|250px]]
|-
| [[File:CSAR20nmoverview+5%.png|250px]]
| [[File:CSAR20nmoverview+10%.png|250px]]
|Platen temperature
|-  
|colspan="2"|20 °C
|-


! rowspan="1" align="center"| Conditions
| Conditioning
|colspan="2"| Pre-clean: 10 min oxygen clean
5 min oxygen clean between runs
|-
! rowspan="2" align="center"| Etch rates
| Si
|colspan="2"|
200 nm lines: ~700 nm/min <br>
130 nm lines: ~580 nm/min <br>


|-
|CSAR
|colspan="2"|  ~18 nm/min
|-
|}
|}

Latest revision as of 08:36, 21 February 2024



Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact lithography at DTU Nanolab.


Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.

Around 2 ml of resist per wafer has been used when fabricating these curves. If you use less than 2 ml, the thickness of the final resist might be smaller than reported here.



AllResist AR-P 6200.09 (> 2ml per 4" wafer) spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm]
2000 4000 226
3000 4000 194
4000 4000 170
5000 4000 151
6000 4000 142
7000 4000 127


AllResist CSAR 6200.09 1:1 in anisole (< 2ml per 4" wafer), Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm]
2000 4000 84
3000 4000 67
4000 4000 59
5000 4000 53
6000 4000 49


AllResist CSAR 6200.18 (< 2ml per 4" wafer), Spin Coater: Manual Standard Resists, E-5, TIGRE, 15-06-2016. Softbake 2 min @ 180 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm]
2000 2000 1003
3000 2000 809
4000 2000 721
5000 2000 639
6000 2000 586
7000 2000 549




Contrast Curve

CSAR 6200.09

100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.

CSAR Contrast Curve, Processed by TIGRE, FEB-MARCH 2016
Resist Spin Coat E-beam exposure Development Characterisation
CSAR AR-P6200.09 AllResist, CSAR AR-P6200.09 diluted 1:1 in Anisole 08-02-2016, LabSpin E-5, 4000 rpm, 60s, softbaked 60s @ 205 degC 09-02-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces 11-02-2016, Fumehood D-2, AR-600-546, rinsed in IPA 60s. 02-03-2016 AFM Icon, F-2, ScanAsyst in Air

AR-P 6200 contrast curves.

Dose to size

Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm2.

Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.

Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.

Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm2. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.

CSAR 6200.18

100 nm lines in ~900 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.

CSAR Contrast Curve, Processed by TIGRE, JUNE 2016
Resist Spin Coat E-beam exposure Development Characterisation
CSAR AR-P6200.18 AllResist 15-06-2016, LabSpin E-5, 2000 rpm, 60s, softbaked 60s @ 205 degC 15-06-2016, JBX9500 E-2, 2nA aperture 5, doses 40-600 µC/cm2, 100 nm lines and 300 nm spaces 16-06-2016, Fumehood E-4, AR-600-546, 30s/60s/90s, rinsed in IPA 60s. JUNE/JULY 2016 SEM Supra 2, 10 keV



Dark Erosion

Dark erosion has been measured on a un-exposed 4" wafer spin coated with CSAR 6200.18 to a thickness of approximately 549 nm. The resist thickness has been measured by VASE Ellipsometer before development, and after 3 minutes, 13 minutes, and 30 minutes of development in AR 600 546.

The graphs shows the measured thicknesses; the errorbars represents the standard deviations from the ellipsometric measurements. The average etch rate of CSAR is ~0.1 nm/min.



Development

Many resists can be developed in different developers, CSAR can be developed in: AR 600-546, AR 600-548, ZED N-50 and mix of MIBK and IPA among others.

CSAR and ZEP520A are in principle the same chemical, however the pretreatment (filtration and temperature control) can differ.

Some users have reported residues and residual layers when using ZED N-50 on CSAR and vice verca, hence we recommend to use AR 600-546 or AR 600-548 (3 times stronger) to develop CSAR and not ZED N-50.

When this is said some users still observe residues when using AR 600-546, the producer "All resist GMBH" have recommended to use 3-5s, dip in pure MIBK to remove residues.

AR 600 546 will dissolve different plastic materials, hence never use it on PS compounds.


Etch Tests

If you have wafers or chips with CSAR you would like to have tested, please send me an [email].

Chlorine versus flourine-based etches

We have experienced problems with removal of CSAR after chlorine-based dry etch, see the file File:DryEtchTestsCSAR.pdf. It seems the chlorine etch forms particles of chlorinated CSAR on the surface, and these particles remains on the surface after resist removal with AR-600-71. The C4F8/SF6 etch also forms particles on the surface, but much smaller than those formed in the chlorine etch. It seems these particles are removed after 3 minutes in AR-600-71.

How to mount chips in dry etch tools

All etch rates presented here are measured on chips (i.e. diced 4" wafers) crystal bonded to a carrier. The carrier is either a blank Si wafer, a Si wafer spin coated with resist or a Si wafer coated with ALD grown Al2O3.

Etch Tests of CSAR, recipe 'nano1.42', DRIE PEGASUS, A-1. CSAR thickness measured on Ellipsometer VASE at 70 degrees
Sample CSAR Etch rate nm/min
Full 4" Si wafer with non-patterned ~180 nm CSAR ~56.5 (based on 2 runs)
Full 4" Si wafer with non-patterned ~240 nm CSAR,
postbaked 60 sec @ 130 degC
~56.5 (based on 2 runs)
1/4 4" Si wafer with non-patterned ~125 nm CSAR,
not crystal bonded to Si carrier
~83.3 (based on 3 runs)
1/4 4" Si wafer with non-patterned ~125 CSAR,
crystal bonded to 4" Si carrier
~54 (based on 1 run)

Etch rates and profile inspection

Continous Etches

Recipe nano1.42 on Deep Reactive Ion Etch PEGASUS A-1
Recipe Gasses C4F8 75 sccm, SF6 38 sccm Profiles of lines exposed at 300 µC/cm2, etched 2:30 minutes (150s) with recipe 'nano1.42'
  
  
Pressure 4 mTorr,

Strike: 3 secs @ 15 mTorr

Power 800 W Coil Power,

40 W Platen Power

Platen temperature - 20°C
Conditions Conditioning Pre-clean: 10 min oxygen clean

5 min oxygen clean between runs

Etch rates Si

500 nm lines: ~200 nm/min
190 nm lines: ~200 nm/min
102 nm lines: ~190 nm/min
61 nm lines: ~170 nm/min

CSAR ~55 nm/min


Recipe processC on Deep Reactive Ion Etch PEGASUS A-1
Recipe Gasses C4F8 70 sccm, SF6 38 sccm Profiles of lines exposed at 300 µC/cm2, etched 60s with recipe 'ProcessC'
 
  
Pressure 4 mTorr,

Strike: secs @ mTorr

Power 450 W Coil Power, 100 W Platen Power
Platen temperature 10°C
Conditions Conditioning Pre-clean: 10 min oxygen clean

5 min oxygen clean between runs

Etch rates Si

500 nm lines: ~300 nm/min
102 nm lines: ~250 nm/min

CSAR 158 nm/min

Bosch Etch

Recipe NBoost01 on Deep Reactive Ion Etch PEGASUS A-1
Recipe Deposition step Duration 2.5 s Profiles of lines exposed at 300 µC/cm2, etched 6:00 minutes with recipe 'NBoost01'
 
 

 
Gasses C4F8 50 sccm, SF6 0 sccm
Pressure 10 mTorr
Powers 500 W Coil
Etch step (boost) Duration 1.5 s
Gasses C4F8 0 sccm, SF6 60 sccm
Pressure 5 mTorr
Powers 400 W Coil, 50 W Platen
Etch step (main) Duration 3.5 s
Gasses C4F8 40 sccm, SF6 60 sccm
Pressure 15 mTorr
Powers 400 W Coil, 20 W Platen
Platen temperature 20 °C
Conditions Conditioning Pre-clean: 10 min oxygen clean

5 min oxygen clean between runs

Etch rates Si

200 nm lines: ~700 nm/min
130 nm lines: ~580 nm/min

CSAR ~18 nm/min