Recipe settings
|
Comments
|
SEM gallery
|
- On 6" wafer
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:25.6
- C4F8 flow [sccm]: 25.6
- He flow [sccm]:448.7
- Pressure:Fully open APC valve (8-9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
text
|
- SiO2 etch with Cr mask on full wafer 6 min etch
|
- Piece on Si carrier
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:25.6
- C4F8 flow [sccm]: 25.6
- He flow [sccm]:448.7
- Pressure:Fully open APC valve (8-9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
More sidewall passivation on chip than on full wafer
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch
|
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- C4F8 flow [sccm]: 25.6
- He flow [sccm]:448.7
- Pressure:Fully open APC valve (8-9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Less sidewall passivation from removing the H2
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm
|
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 5
- C4F8 flow [sccm]: 25.6
- He flow [sccm]:448.7
- Pressure:Fully open APC valve (8-9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Not a large effect from adding a little O2
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, O2:5sccm
|
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 0
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:225
- Pressure:Fully open APC valve (3.35 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Reducing total flow rate and thereby the pressure gives less passivation/redeposition. Sidewall roughness not so bad.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr
|
- Coil Power [W]:1200
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 0
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:225
- Pressure:Fully open APC valve (3.35 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Reducing the coil power a lot and platen power a little gives more sidewall passivation/redeposition
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W
|
- Coil Power [W]:1200
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:215
- Pressure:Fully open APC valve (3.35 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Adding oxygen reduces the passivation/redeposition
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
|
- Coil Power [W]:1200
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.35 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Adding more oxygen reduces further the passivation/redeposition but some trenching appears.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
|
- Coil Power [W]:1800
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:215
- Pressure:Fully open APC valve (3.35 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Increasing coil power reduces trenching but increases passivation/redeposition
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
|
- Coil Power [W]:1800
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.6 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Adding more O2 reduces the sidewall passivation/redeposition
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
pitch 800 nm Top 461 nm @edge 437 nm bottom 402 nm height 916 nm height from edge 827 nm Cr left 83.5 nm selectivity 55.5
|
- Coil Power [W]:1200
- Platen Power [W]: 100
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.6 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Running with the lower coil power and reducing the platen power also seems to reduced the sidewall passivatin/redeposition, but etch rate goes down
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
pitch 800 nm Top 444 nm bottom 374 nm height 718 nm Cr left 85 nm selectivity 48
|
- Coil Power [W]:1200
- Platen Power [W]: 100
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.6 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Repeating with longer etch time to etch 1500 nm down. Unfortunately this damaged the hardware due to the EM coils getting too hot.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT THIS LONG TIME), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
Etch on none patterned wafer, Uniformity: +- 6.4%
|
- Coil Power [W]:1800
- Platen Power [W]: 150
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.6 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
- PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|
Running 1800W/150W at increased time to etch down to 1500 nm.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
|
- Coil Power [W]:1200
- Platen Power [W]: 100
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
Repeating the 1200W/100W recipes at 14 min but without the EM coils. For this recipe the uniformity over the wafer improved from removing the EM coils, so no need for those and now the recipe could run 14 min without damaging the hardware. The profile looked as before. After removing the Cr I looked from the top and with a tilted view and saw the the sidewall roughness was very bad.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.9mTorr; platen power 100W, coil power:1200W
Etch on none patterned wafer, Uniformity: +-1.7%
|
- Coil Power [W]:2500
- Platen Power [W]: 100
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
Tried high coil power and low platen power. This seemed to give som undercutting,especially on the narrow lines. The smallest has been etched away.
|
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.9mTorr; platen power 100W, coil power:2500W
|
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 0
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:225
- Pressure:Fully open APC valve (3.9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:225sccm O2:0sccm, Pressure:3.9mTorr; platen power 200W, coil power:2500W
|
- 14 min
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 20
- C4F8 flow [sccm]: 13.0
- He flow [sccm]:205
- Pressure:Fully open APC valve (3.9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.9mTorr; platen power 200W, coil power:2500W
|
- Back to start setting without EM coils - 14 min
- Coil Power [W]:2500
- Platen Power [W]: 200
- Platen temperature [oC]: 20
- H2 flow [sccm]:25.6
- O2 flow [sccm]: 0
- C4F8 flow [sccm]: 25.6
- He flow [sccm]:448.7
- Pressure:Fully open APC valve (8-9 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0
|
- Coil Power [W]:600
- Platen Power [W]: 50
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 6.5
- He flow [sccm]:100
- Pressure:Fully open APC valve (<2 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- C10751: SiO2 etch with Cr mask on wafer piece on Si carrier 20 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 50W, coil power:600W
|
- Coil Power [W]:300
- Platen Power [W]: 25
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 6.5
- He flow [sccm]:100
- Pressure:Fully open APC valve (<2 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- C10752: SiO2 etch with Cr mask on wafer piece on Si carrier 30 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W
|
- 45 min
- Coil Power [W]:300
- Platen Power [W]: 25
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 6.5
- He flow [sccm]:100
- Pressure:Fully open APC valve (<2 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- C10834: SiO2 etch with Cr mask on wafer piece on Si carrier 45 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W
|
- Coil Power [W]:300
- Platen Power [W]: 20
- Platen temperature [oC]: 20
- H2 flow [sccm]:0
- O2 flow [sccm]: 10
- C4F8 flow [sccm]: 6.5
- He flow [sccm]:100
- Pressure:Fully open APC valve (<2 mTorr)
- Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|
|
text
- C10844: SiO2 etch with Cr mask on wafer piece on Si carrier 50 min etch, EM:0/0 H2:0sccm, C4F8:6.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 20W, coil power:300W
|