Specific Process Knowledge/Thin film deposition/Deposition of Aluminium/Thermal deposition of Al: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
 
(20 intermediate revisions by 3 users not shown)
Line 1: Line 1:




'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium/Thermal_deposition_of_Al click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium/Thermal_deposition_of_Al click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin film deposition/Deposition of Aluminum" with the link to the Labadviser page-->


''All text on this page by DTU Nanolab staff''


== '''Thermal evaporation of Aluminum''' ==
== '''Thermal evaporation of Aluminum''' ==


Aluminum can be thermally evaporated in the [[Specific Process Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]] and the [[Specific Process Knowledge/Thin_film_deposition/Wordentec|Wordentec]]. At DTU Danchip, we recommend to use a thin layer of thermally evaporated aluminum on top of e-beam resist, before the e-beam exposure.
Aluminum can be thermally evaporated in the [[Specific Process Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]] and the [[Specific Process Knowledge/Thin_film_deposition/Wordentec|Wordentec]]. At DTU Nanolab, we recommend to use a thin layer of thermally evaporated aluminum on top of e-beam resist before the e-beam exposure.
For deposition onto the unexposed e-beam resist, you need to use the thermal source.  
For deposition onto the unexposed e-beam resist, you need to use the thermal source.


===Using the Thermal Evaporator===
== Using the Thermal Evaporator ==


The Thermal Evaporator (Lesker) is easy to use and the quickest option if you only have a few samples or several small samples. It is also better suited for depositing rather thick layers, since you can add more material and the material use is more efficient than in the Wordentec. However, the deposited thickness will vary more across a large wafer than in the Wordentec because the throw distance is shorter.
The Thermal Evaporator (Lesker) is easy to use and the quickest option if you only have a few samples or several small samples. It is also better suited for depositing rather thick layers, since you can add more material and the material use is more efficient than in the Wordentec. However, the deposited thickness will vary more across a large wafer than in the Wordentec because the throw distance is shorter (4-14 % variation across a 4" wafer for the Thermal Evaporator versus 3-6 % variation across a 4" wafer with the Wordentec).
 
See a few more details comparing the instruments including particle count and uniformity on 6" wafers here:
[[:File:thermal evap wtec vs lesker nano uniformity and particles.pdf]]
 
Notice that since this measurement was made we have implemented rotation in the machine, so it may be better now (June 2023).


As usual, you need a training session before using the instrument independently.
As usual, you need a training session before using the instrument independently.
Line 24: Line 29:
For Al-deposition, you must activate source no. 1 and choose a process starting with "Al1". Follow the directions in the manual.
For Al-deposition, you must activate source no. 1 and choose a process starting with "Al1". Follow the directions in the manual.


===Using the Wordentec===
===Quality control (QC) of Al evaporation on the thermal evaporator===
 
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality control (QC) for the Thermal evaporator'''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=6654&mach=404 QC procedure for the Thermal Evaporator]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=404 The newest QC data for the Thermal evaporator]<br>
 
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:400px"
 
! QC Recipe:
! Al1_1A/s
|-
|Deposition rate
|1 Å/s
|-
|Thickness
|150 nm
|-
|Pressure
|Below 1*10<sup>-5</sup> Torr
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:440px"
!QC limits
!Thermal Evaporator
|-
|Measured average thickness
|± 20 %
|-
|Deposition rate deviation
|± 50 % after stabilizing
|-
|Thickness deviation across a 4" wafer
|± 30 %
|-
|}
|-
|}
Thicknesses are measured in 5 points with one of the stylus profilers. <br>
Additionally we monitor the pumpdown time and the state of the Al crucible and ensure that it does not contain too much Al as this can wet the outside and short circuit the heater.
|}
 
<br clear="all" />
 
[[Image:Lesker 02.tif|700px|thumb|left|100nm Al deposited by Thermal evaporator/ SEM image was taken by Patama Pholprasit]]


The Wordentec is useful if you need to deposit a thin layer on more than three wafers: You can load up to six 6" wafers at a time, but you can only add 8 pellets at a time, which in the Wordentec gives a ''total'' of approx. 150 nm (or 20 nm per wafer on six wafers, as extra material is used up for each soaking step). The pumping time for the Wordentec is at least 1 hour, which means that this is much slower than the Thermal Evaporator unless you are depositing on many wafers. The deposited thickness will be much more uniform across a 4" or 6" wafer in the Wordentec than in the Thermal Evaporator (see measured uniformity on the instrument pages for the Wordentec and the Thermal Evaporator).
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
 
==Using the Wordentec==
 
The Wordentec is useful if you need to deposit a thin layer on more than three wafers: You can load up to six 6" wafers at a time, but you can only add 8 pellets at a time, which in the Wordentec gives a ''total'' of approx. 150 nm (or 20 nm per wafer on six wafers, as extra material is used up for each soaking step). The pumping time for the Wordentec is at least 1 hour, which means that this is much slower than the Thermal Evaporator unless you are depositing on many wafers.  


Use '''process 9''' in Wordentec to deposit thermal Aluminum. Follow the manual.
Use '''process 9''' in Wordentec to deposit thermal Aluminum. Follow the manual.
Line 57: Line 160:
=====Notes=====
=====Notes=====
This files contains some short notes regarding thermal Al evaporation: [[media: Notes_from_test_with_thermal_evaporation_source.pdf‎|Short Tests thermal deposition of Al in Wordentec]]
This files contains some short notes regarding thermal Al evaporation: [[media: Notes_from_test_with_thermal_evaporation_source.pdf‎|Short Tests thermal deposition of Al in Wordentec]]
[[File:Wordentec_00.tif|700px|thumb|left|100nm Al film deposited by Thermal process in Wordentec/ SEM image was taken by Patama Pholprasit]]

Latest revision as of 14:13, 25 January 2024


Feedback to this page: click here

All text on this page by DTU Nanolab staff

Thermal evaporation of Aluminum

Aluminum can be thermally evaporated in the Thermal Evaporator and the Wordentec. At DTU Nanolab, we recommend to use a thin layer of thermally evaporated aluminum on top of e-beam resist before the e-beam exposure. For deposition onto the unexposed e-beam resist, you need to use the thermal source.

Using the Thermal Evaporator

The Thermal Evaporator (Lesker) is easy to use and the quickest option if you only have a few samples or several small samples. It is also better suited for depositing rather thick layers, since you can add more material and the material use is more efficient than in the Wordentec. However, the deposited thickness will vary more across a large wafer than in the Wordentec because the throw distance is shorter (4-14 % variation across a 4" wafer for the Thermal Evaporator versus 3-6 % variation across a 4" wafer with the Wordentec).

See a few more details comparing the instruments including particle count and uniformity on 6" wafers here: File:thermal evap wtec vs lesker nano uniformity and particles.pdf

Notice that since this measurement was made we have implemented rotation in the machine, so it may be better now (June 2023).

As usual, you need a training session before using the instrument independently.

To deposit Al
  • Vent the chamber (3 min)
  • Load your sample(s) and add Al pellets to the crucible as necessary (you need approx. 1 pellet per 45 nm, note that there may also be some Al left in the crucible)
  • Pump down (10 min)
  • Run the process (soaking/ramping 7 minutes plus time for your deposition and about 1 minute for running down the power afterwards). The deposition rate is 1 Å/s.

For Al-deposition, you must activate source no. 1 and choose a process starting with "Al1". Follow the directions in the manual.

Quality control (QC) of Al evaporation on the thermal evaporator

Quality control (QC) for the Thermal evaporator
QC Recipe: Al1_1A/s
Deposition rate 1 Å/s
Thickness 150 nm
Pressure Below 1*10-5 Torr
QC limits Thermal Evaporator
Measured average thickness ± 20 %
Deposition rate deviation ± 50 % after stabilizing
Thickness deviation across a 4" wafer ± 30 %

Thicknesses are measured in 5 points with one of the stylus profilers.
Additionally we monitor the pumpdown time and the state of the Al crucible and ensure that it does not contain too much Al as this can wet the outside and short circuit the heater.


100nm Al deposited by Thermal evaporator/ SEM image was taken by Patama Pholprasit

























Using the Wordentec

The Wordentec is useful if you need to deposit a thin layer on more than three wafers: You can load up to six 6" wafers at a time, but you can only add 8 pellets at a time, which in the Wordentec gives a total of approx. 150 nm (or 20 nm per wafer on six wafers, as extra material is used up for each soaking step). The pumping time for the Wordentec is at least 1 hour, which means that this is much slower than the Thermal Evaporator unless you are depositing on many wafers.

Use process 9 in Wordentec to deposit thermal Aluminum. Follow the manual.

Observe that you need to get a special training to use the thermal deposition source.

Set-up
  • Two "boats" of Tantalum are mounted (on top of each other) in the thermal source each time.
    • We have also earlier seen that two boats give stable depositions, since the lower boat gets hot (and heat the top boat), even if there if a thick layer of aluminum all over the top boat.

  • If the last deposition from the source was Aluminum, the same boats can be used, otherwise they should be changed.
  • "Small" Al pellets (diameter 1/8", height 1/8") are used. Use these small pellets to get a more uniform deposition with stable deposition rate.
  • The boat should be placed as horizontal as possible, so the Aluminum metal will be evenly distributed in the boat after it is melted. If it is a problem to mount the boats horizontal, contact equipment responsible persons.
Program settings
  • The deposition rate is normally 1 or 2 Å/s.

The settings saved in the material file for thermal aluminum are these:

  • Soak power 1: 5%
  • Soak power 2: 7%

These are already saved in the process recipe.

Notes

This files contains some short notes regarding thermal Al evaporation: Short Tests thermal deposition of Al in Wordentec


100nm Al film deposited by Thermal process in Wordentec/ SEM image was taken by Patama Pholprasit