Specific Process Knowledge/Characterization/Topographic measurement: Difference between revisions
(26 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:Characterization@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php | '''Feedback to this page''': '''[mailto:Characterization@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/Topographic_measurement click here]''' | ||
=Topographic measurements= | |||
Topographic measurements are measurements of height differences on your sample. If you measure many spots on the sample you can get a topographic image of the surface. | |||
At DTU Nanolab we have eight systems for topographic measurements: | |||
*Stylus profilers (P17, Dektak XTA, Dektak 150 and Dektak 3ST) - ''Profilers for measuring micro structures'' | |||
*Optical profilers (Optical profiler Sensofar and Optical profiler Filmetrics) - ''3D Profilers for measuring micro structures'' | |||
*AFMs (AFM Icon-PT1 and AFM Icon-PT2) - ''AFMs for measuring nano structures'' | |||
==High aspect ratio structures== | |||
The fact that the stylus tip of a stylus profiler or an AFM is shaped like a cone with some finite tip angle causes a problem when characterizing high aspect ratio structures. For instance, if a 20 µm wide trench is etched deeper than approximately 18 µm, the tip of the Dektak will not be able to reach the bottom. The optical profiler uses a light beam that is focused through an objective. Therefore it is able to measure higher aspect ratios. The aspect ratio is limited by the possibility for the light to reach the bottom and get back to the detector. On some samples we have been able to measure aspect ratios above 1:10. Otherwise the solution is to cleave the sample along a line that is perpendicular to the trench and then inspect the profile in a [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy|scanning electron microscope]] or a microscope (for large structures). | |||
==Thin film thickness== | |||
The | The profilers can be used to measure the thickness of optically transparent thin films or etched non-transparent thin films. There are also other options for measuring film thickness. All the methods are compared on the [[Specific Process Knowledge/Characterization/Measurement of film thickness and optical constants| "Measurement of thin film thickness and optical constants"]] page | ||
==Comparison of stylus profilers, optical profilers and AFMs at Nanolab== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
Line 21: | Line 23: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Characterization/Profiler# | ![[Specific Process Knowledge/Characterization/Profiler#P17_stylus_profiler|P17 stylus profiler]] | ||
![[Specific Process Knowledge/Characterization/Profiler#Dektak XTA_new_stylus_profiler|Dektak | ![[Specific Process Knowledge/Characterization/Profiler#Dektak XTA_new_stylus_profiler|Dektak XTA stylus profiler]] | ||
![[Specific Process Knowledge/Characterization/Profiler#Optical_Profiler_(Sensofar)|Optical Profiler (Sensofar)]] | ![[Specific Process Knowledge/Characterization/Profiler#Optical_Profiler_(Sensofar)|Optical Profiler (Sensofar)]] | ||
![[Specific Process Knowledge/Characterization/Profiler#Optical_Profiler_(Filmetrics)|Optical Profiler (Filmetrics)]] | ![[Specific Process Knowledge/Characterization/Profiler#Optical_Profiler_(Filmetrics)|Optical Profiler (Filmetrics)]] | ||
![[Specific Process Knowledge/Characterization/AFM: Atomic Force Microscopy|AFM Icon]] | ![[Specific Process Knowledge/Characterization/AFM: Atomic Force Microscopy|AFM Icon 1 and AFM Icon 2]] | ||
![[Specific Process Knowledge/Characterization/Profiler#Dektak III-V Profiler|Dektak 3ST]] | ![[Specific_Process_Knowledge/Characterization/Profiler#Stylus_Profiler:_Dektak150|Dektak 150 stylus profiler]] | ||
![[Specific Process Knowledge/Characterization/Profiler#Dektak III-V Profiler|Dektak 3ST stylus profiler]] | |||
|- | |- | ||
Line 32: | Line 35: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Profiler for measuring | |Profiler for measuring microstructures. Excellent stress measurements. Excellent sequence programs. Also wafer mapping and roughness measurements. | ||
|Profiler for measuring | |Profiler for measuring microstructures. Quick and easy vertical profiling. Also wafer mapping, roughness and stress measurements. | ||
|3D Profiler for measuring | |3D Profiler for measuring microstructures and surface roughness. Can do wafer mapping. | ||
|3D Profiler for measuring | |3D Profiler for measuring microstructures and surface roughness. Can do wafer mapping. Located in the basement. | ||
|AFM for measuring nanostructures and surface roughness | |AFM for measuring nanostructures and surface roughness | ||
|Profiler for measuring | |Profiler for measuring microstructures. Located in building 451, room 913. | ||
|Profiler for measuring microstructures. Located in the basement. | |||
|- | |- | ||
Line 43: | Line 47: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!'''Max. scan range xy''' | !'''Max. scan range xy''' | ||
|Line scan x: | |Line scan x: 1 µm to 200mm. | ||
|Line scan x: 50µm to 55mm in one scan. Maximum scan | Map scan xy: up to the largest square that can be inscribed in an 8" wafer | ||
|Line scan x: 50µm to 55mm in one scan. Maximum scan length with stitching 200mm. | |||
|Depending on the objective: | |Depending on the objective: | ||
*One view: 127µmX95µm to 1270µmX955µm | *One view: 127µmX95µm to 1270µmX955µm | ||
*Stitching: In principel a | *Stitching: In principel a whole 6" wafer (time consuming) | ||
|Only 10x objective: | |Only 10x objective: 2.0 mm x 1.7 mm | ||
|90 µm square | |90 µm square | ||
|Line scan x: 50-55000 µm | |||
|Line scan x: 50-50000 µm | |Line scan x: 50-50000 µm | ||
|- | |- | ||
Line 56: | Line 62: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!'''Max. scan range z''' | !'''Max. scan range z''' | ||
| | |up to 900 µm | ||
| | |50 Å to 1 mm | ||
|Depending on the objective and Z resolution: | |Depending on the objective and Z resolution: | ||
*94.4 µm ->9984 µm | *94.4 µm ->9984 µm | ||
|10 mm (piezo range 500 µm) | |10 mm (piezo range 500 µm) | ||
|1 µm (can go up to 5 µm under special settings) | |1 µm (can go up to 5 µm under special settings) | ||
|130 nm | |50 Å to 1 mm | ||
|100 Å to 130 nm | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!'''Resolution xy''' | !'''Resolution xy''' | ||
|down to 0. | |down to 0.025 µm | ||
|down to 0.003 µm | |down to 0.003 µm | ||
|Depending on the objective: | |Depending on the objective: | ||
*0.5µm -> 5µm | *0.5µm -> 5µm | ||
| | |Resolving power of the lens: 0.92 µm | ||
|Depending on scan size and number of samples per line and number of lines - accuracy better than 2% | |Depending on scan size and number of samples per line and number of lines - accuracy better than 2% | ||
| | |down to 0.003 µm | ||
|down to 0.5 µm | |||
|- | |- | ||
Line 78: | Line 86: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!'''Resolution z''' | !'''Resolution z''' | ||
| | |0.01, 0.08 or 0.6 Å depending on range (note resolution much below 1 Å is not so useful since it is far below the noise level) | ||
| | |1 Å, 10 Å, 40 Å or 160 Å depending on range | ||
|Depending on measuring methode: | |Depending on measuring methode: | ||
*PSI down to 0.01 nm | *PSI down to 0.01 nm | ||
Line 85: | Line 93: | ||
*Confocal (depending on objective): 1nm -> 50nm | *Confocal (depending on objective): 1nm -> 50nm | ||
| | | | ||
* | *Accuracy 0.7% | ||
* | *Precision 0.1% | ||
|<1Å - accuracy better than 2% | |<1Å - accuracy better than 2% | ||
| | |1 Å, 10 Å or 20 Å depending on range | ||
|1 Å, 10 Å, 40 Å or 160 Å depending on range | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!'''Max. scan depth [µm] | !'''Max. scan depth [µm] as a function of trench width W''') | ||
| | |0.866*(W[µm]-2µm) | ||
|1.2*(W[µm]-5µm) | |1.2*(W[µm]-5µm) | ||
|Depending on material and trench width: | |Depending on material and trench width: | ||
*Somewhere between 1:1 and 1:12 | *Somewhere between 1:1 and 1:12 | ||
| | |Depending on material and trench width. | ||
|~1:1 with standard cantilever. | |~1:1 with standard cantilever. | ||
| | |1.2*(W[µm]-5µm) | ||
|1.2*(W[µm]-2.5µm) | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!''' | !'''Standard tip radius''' | ||
| | |2 µm 60<sup>o</sup> cone | ||
|5 µm 45<sup>o</sup> cone | |5 µm 45<sup>o</sup> cone | ||
|No tip - using light | |No tip - using light | ||
Line 113: | Line 123: | ||
*White broadband LED: 550nm | *White broadband LED: 550nm | ||
|<12 nm on standard cantilever | |<12 nm on standard cantilever | ||
| | |5 µm 45<sup>o</sup> cone | ||
|2.5 µm 45<sup>o</sup> cone | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!'''Stress measurement''' | !'''Stress measurement''' | ||
| | |Excellent capability | ||
|Can be done | |Can be done | ||
|No stress calculation capability | |No stress calculation capability | ||
|Cannot be done | |||
|Cannot be done | |Cannot be done | ||
|Cannot be done | |Cannot be done | ||
Line 129: | Line 141: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!'''Surface roughness''' | !'''Surface roughness''' | ||
|Can be done on a line | |Can be done on a line or map (parallel line scans) | ||
|Can be done on a line scan | |Can be done on a line scan | ||
|Can be done on a line or an area | |Can be done on a line or an area | ||
|Can be done on a line or an area | |Can be done on a line or an area | ||
|Can be done on a selected surface area | |Can be done on a selected surface area | ||
|Recommended to use Dektak XTA | |Can be done on a line scan | ||
|Recommended to use P17 or Dektak XTA | |||
|- | |- | ||
Line 145: | Line 158: | ||
|100x100 mm | |100x100 mm | ||
|6" or less | |6" or less | ||
|up to 6" | |||
|4" or less | |4" or less | ||
|- | |- | ||
Line 161: | Line 175: | ||
| | | | ||
*Almost any material that does not leave residual on the stage, please check the responsible group for any non standard materials | *Almost any material that does not leave residual on the stage, please check the responsible group for any non standard materials | ||
| | |||
*Almost any material that does not leave residual on the stage. | |||
| | | | ||
*Almost any material that does not leave residual on the stage. | *Almost any material that does not leave residual on the stage. | ||
|- | |- | ||
|- | |||
|-style="background:LightGrey; color:black" | |||
!'''Location''' | |||
|Cleanroom F-2 | |||
|Cleanroom B-1 | |||
|Cleanroom C-1 | |||
|Basement, building 346, room 904 | |||
|AFM Icon1: Cleanroom C-1 | |||
AFM Icon2: Basement, building 346, room 904 | |||
|Temporary lab in building 451, room 913 | |||
|Basement, building 346, room 904 | |||
|- | |||
|} | |} |
Latest revision as of 12:40, 22 January 2024
Feedback to this page: click here
Topographic measurements
Topographic measurements are measurements of height differences on your sample. If you measure many spots on the sample you can get a topographic image of the surface.
At DTU Nanolab we have eight systems for topographic measurements:
- Stylus profilers (P17, Dektak XTA, Dektak 150 and Dektak 3ST) - Profilers for measuring micro structures
- Optical profilers (Optical profiler Sensofar and Optical profiler Filmetrics) - 3D Profilers for measuring micro structures
- AFMs (AFM Icon-PT1 and AFM Icon-PT2) - AFMs for measuring nano structures
High aspect ratio structures
The fact that the stylus tip of a stylus profiler or an AFM is shaped like a cone with some finite tip angle causes a problem when characterizing high aspect ratio structures. For instance, if a 20 µm wide trench is etched deeper than approximately 18 µm, the tip of the Dektak will not be able to reach the bottom. The optical profiler uses a light beam that is focused through an objective. Therefore it is able to measure higher aspect ratios. The aspect ratio is limited by the possibility for the light to reach the bottom and get back to the detector. On some samples we have been able to measure aspect ratios above 1:10. Otherwise the solution is to cleave the sample along a line that is perpendicular to the trench and then inspect the profile in a scanning electron microscope or a microscope (for large structures).
Thin film thickness
The profilers can be used to measure the thickness of optically transparent thin films or etched non-transparent thin films. There are also other options for measuring film thickness. All the methods are compared on the "Measurement of thin film thickness and optical constants" page
Comparison of stylus profilers, optical profilers and AFMs at Nanolab
P17 stylus profiler | Dektak XTA stylus profiler | Optical Profiler (Sensofar) | Optical Profiler (Filmetrics) | AFM Icon 1 and AFM Icon 2 | Dektak 150 stylus profiler | Dektak 3ST stylus profiler | |
---|---|---|---|---|---|---|---|
Generel description | Profiler for measuring microstructures. Excellent stress measurements. Excellent sequence programs. Also wafer mapping and roughness measurements. | Profiler for measuring microstructures. Quick and easy vertical profiling. Also wafer mapping, roughness and stress measurements. | 3D Profiler for measuring microstructures and surface roughness. Can do wafer mapping. | 3D Profiler for measuring microstructures and surface roughness. Can do wafer mapping. Located in the basement. | AFM for measuring nanostructures and surface roughness | Profiler for measuring microstructures. Located in building 451, room 913. | Profiler for measuring microstructures. Located in the basement. |
Max. scan range xy | Line scan x: 1 µm to 200mm.
Map scan xy: up to the largest square that can be inscribed in an 8" wafer |
Line scan x: 50µm to 55mm in one scan. Maximum scan length with stitching 200mm. | Depending on the objective:
|
Only 10x objective: 2.0 mm x 1.7 mm | 90 µm square | Line scan x: 50-55000 µm | Line scan x: 50-50000 µm |
Max. scan range z | up to 900 µm | 50 Å to 1 mm | Depending on the objective and Z resolution:
|
10 mm (piezo range 500 µm) | 1 µm (can go up to 5 µm under special settings) | 50 Å to 1 mm | 100 Å to 130 nm |
Resolution xy | down to 0.025 µm | down to 0.003 µm | Depending on the objective:
|
Resolving power of the lens: 0.92 µm | Depending on scan size and number of samples per line and number of lines - accuracy better than 2% | down to 0.003 µm | down to 0.5 µm |
Resolution z | 0.01, 0.08 or 0.6 Å depending on range (note resolution much below 1 Å is not so useful since it is far below the noise level) | 1 Å, 10 Å, 40 Å or 160 Å depending on range | Depending on measuring methode:
|
|
<1Å - accuracy better than 2% | 1 Å, 10 Å or 20 Å depending on range | 1 Å, 10 Å, 40 Å or 160 Å depending on range |
Max. scan depth [µm] as a function of trench width W) | 0.866*(W[µm]-2µm) | 1.2*(W[µm]-5µm) | Depending on material and trench width:
|
Depending on material and trench width. | ~1:1 with standard cantilever. | 1.2*(W[µm]-5µm) | 1.2*(W[µm]-2.5µm) |
Standard tip radius | 2 µm 60o cone | 5 µm 45o cone | No tip - using light
|
No tip - using light
|
<12 nm on standard cantilever | 5 µm 45o cone | 2.5 µm 45o cone |
Stress measurement | Excellent capability | Can be done | No stress calculation capability | Cannot be done | Cannot be done | Cannot be done | Cannot be done |
Surface roughness | Can be done on a line or map (parallel line scans) | Can be done on a line scan | Can be done on a line or an area | Can be done on a line or an area | Can be done on a selected surface area | Can be done on a line scan | Recommended to use P17 or Dektak XTA |
Substrate size | up to 8" | up to 6" | Up to more than 6" | 100x100 mm | 6" or less | up to 6" | 4" or less |
Allowed materials |
|
|
|
|
|
|
|
Location | Cleanroom F-2 | Cleanroom B-1 | Cleanroom C-1 | Basement, building 346, room 904 | AFM Icon1: Cleanroom C-1
AFM Icon2: Basement, building 346, room 904 |
Temporary lab in building 451, room 913 | Basement, building 346, room 904 |