Recipes and results - CHF3 tests
Tests performed with AZ5214E resist:
Recipe
|
Recipe parameters
|
Process time
|
Date
|
SEM picture
|
SEM pic w/ no resist
|
Redeposition - top view
|
Profile angles
|
Etch rate in SiO2
|
Etch rate in resist (AZ5214E inverse)
|
Selectivity (SiO2:resist)
|
Etch rate in Si
|
CHF3_t1
|
CHF3= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
12:00 min
|
04/09/2023
|
|
|
|
|
69.7 nm/min +/- 10.5%
|
57.3 nm/min +/- 12.9%
|
1.22
|
|
CHF3_t2
|
CHF3= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
25:00 min
|
04/09/2023
|
|
|
|
|
26.7 nm/min +/- 11.9%
|
24.2 nm/min +/- 21.1%
|
1.1
|
|
CHF3 t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
9,7 nm/min +/- 34.4%
|
1,8 nm/min +/- 46.5%
|
5.4
|
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
12/09/2023
|
|
|
|
|
59,6 nm/min +/- 12.9%
|
47,5 nm/min +/- 21.5%
|
1.25
|
|
CHF3_t1
|
CHF3= 22.5 sccm O2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
11/09/2023
|
|
|
|
|
60,6 nm/min +/- 10.1%
|
130,8 nm/min +/- 8.8%
|
0.46
|
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
20/09/2023
|
|
|
|
|
47,3 nm/min +/- 12%
|
26,4 nm/min +/- 17,4%
|
1.8
|
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
36,5 nm/min +/- 10.6%
|
17,5 nm/min +/- 13.9%
|
2.09
|
|
CHF3 t1
|
CHF3= 35 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
42 nm/min +/- 15.4%
|
23,8 nm/min +/- 22.2%
|
1.76
|
|
CHF3 t1
|
CHF3= 22.5 sccm CF4= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
75,8 nm/min +/- 13.1%
|
74,9 nm/min +/- 10.8%
|
1.01
|
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 25mTorr Temp= 20°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
-
|
-
|
no etch done, polymer deposited
|
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 0°C
|
10:00 min
|
22/09/2023
|
|
|
|
|
48 nm/min +/- 11.2%
|
23,3 nm/min +/- 13.7%
|
2.06
|
|
Tests performed with 915nm UVN resist + 88nm BARC:
Recipe
|
Recipe parameters
|
Process time
|
Date
|
SEM picture
|
SEM pic w/ no resist
|
Redeposition - top view
|
Profile angles
|
Etch rate in SiO2
|
Etch rate in resist (AZ5214E inverse)
|
Selectivity (SiO2:resist)
|
Etch rate in Si
|
CHF3_t1
|
CHF3= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
12:00 min
|
04/09/2023
|
|
|
|
|
69.7 nm/min +/- 10.5%
|
57.3 nm/min +/- 12.9%
|
1.22
|
|
CHF3_t2
|
CHF3= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
25:00 min
|
04/09/2023
|
|
|
|
|
26.7 nm/min +/- 11.9%
|
24.2 nm/min +/- 21.1%
|
1.1
|
|