Line 213: |
Line 213: |
|
| |
|
| ===Profile, top view at tilted SEM images=== | | ===Profile, top view at tilted SEM images=== |
| <gallery caption="SiO2 etch with Cr mask on full wafer 6 min etch" perrow="6" widths="400px" heights="300px"> | | <gallery caption="SiO2 etch with Cr mask on full wafer 6 min etch" perrow="4" widths="400px" heights="300px"> |
|
| |
|
|
| |
|
Line 220: |
Line 220: |
| </gallery> | | </gallery> |
|
| |
|
| <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch" perrow="6" widths="200px" heights="150px"> | | <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch" perrow="4" widths="400px" heights="300px"> |
|
| |
|
| File:C10022_03__02.jpg | | File:C10022_03__02.jpg |
Line 238: |
Line 238: |
| </gallery> | | </gallery> |
|
| |
|
| <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr" perrow="6" widths="200px" heights="150px"> | | <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr" perrow="4" widths="400px" heights="300px"> |
|
| |
|
| File:C10082_07.jpg | | File:C10082_07.jpg |
Revision as of 14:20, 3 November 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
SiO2 trench etching with Cr mask
Start parameters, variations noted in the gallery headline
|
Recipe name: no 10 with lower platen power
|
Coil Power [W]
|
2500
|
Platen Power [W]
|
200
|
Platen temperature [oC]
|
20
|
H2 flow [sccm]
|
25.6
|
C4F8 flow [sccm]
|
25.6
|
He flow [sccm]
|
448.7
|
Pressure
|
Fully open APC valve (8-9 mTorr)
|
Electromagnetic coils (EM) 'outer coil' / 'inner coil'
|
'2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN)
|
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Results
Temporary conclusions on how the process parameters affect the results in this study:
|
What process parameters affect the results?
|
- Going from full wafer to small piece on Si carrier:
- Seemed to give more sidewall passivation
- Platen power: lowering the platen power gives
- more sidewall passivation
- lower etch rate
- Less trenching
- Removing the H2 gave:
- less sidewall passivation
- Adding O2 gave:
- less sidewall passivation
- Process pressure/total gasflow rate
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- less sidewall passivation
- Reduced the CD (Critical Dimensions)
- Coil power: Reducing coil power
- less CD loss
- more sidewall passivation
- Increasing process time:
- less sidewall passivation
- more sidewall bow
- CD loss due to larger mask faceting
|
- Sidewall passivation↑
- Sample size↓
- Platen power↓
- Coil power↓
- H2 flow↑
- O2 flow↓
- Total gas flow rate/pressure↑
|
Profile SEM images
- SiO2 etch with Cr mask on full wafer 6 min etch
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, O2:5sccm
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
-
-
-
-
-
Profile, top view at tilted SEM images
- SiO2 etch with Cr mask on full wafer 6 min etch
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, O2:5sccm
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT THIS LONG TIME), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.9mTorr; platen power 100W, coil power:1200W
-
-
-
-
-
-
-