Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions
No edit summary |
No edit summary |
||
Line 79: | Line 79: | ||
|- | |- | ||
|} | |} | ||
====Profile SEM images==== | |||
<gallery caption="SiO2 etch with Cr mask on full wafer 6 min etch" perrow="6" widths="200px" heights="150px"> | <gallery caption="SiO2 etch with Cr mask on full wafer 6 min etch" perrow="6" widths="200px" heights="150px"> | ||
Line 210: | Line 210: | ||
File:Contour Plot Y33 EM_0_0 blue to red.jpg| Etch on none patterned wafer, Uniformity: +-1.7% | File:Contour Plot Y33 EM_0_0 blue to red.jpg| Etch on none patterned wafer, Uniformity: +-1.7% | ||
</gallery> | </gallery> | ||
====Profile, top view at tilted SEM images==== |
Revision as of 11:12, 3 November 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
Start parameters, variations noted in the gallery headline | Recipe name: no 10 with lower platen power |
---|---|
Coil Power [W] | 2500 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
H2 flow [sccm] | 25.6 |
C4F8 flow [sccm] | 25.6 |
He flow [sccm] | 448.7 |
Pressure | Fully open APC valve (8-9 mTorr) |
Electromagnetic coils (EM) 'outer coil' / 'inner coil' | '2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN) |
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Results
Temporary conclusions on how the process parameters affect the results in this study: | What process parameters affect the results? |
|
|
Profile SEM images
-
pitch 800 nm
Top 461 nm
@edge 437 nm
bottom 402 nm
height 916 nm
height from edge 827 nm
Cr left 83.5 nm
selectivity 55.5 -
156 nm/min
-
pitch 800 nm
Top 444 nm
bottom 374 nm
height 718 nm
Cr left 85 nm
selectivity 48
-
Etch on none patterned wafer, Uniformity: +- 6.4%
-
Etch on none patterned wafer, Uniformity: +-1.7%