Line 189: |
Line 189: |
| File:C10160_15.jpg | | File:C10160_15.jpg |
| File:C10160_17.jpg | | File:C10160_17.jpg |
| File:Contour Plot Y32 EM_02_30 blue to red.jpg | | File:Contour Plot Y32 EM_02_30 blue to red.jpg| Uniformity: +- 6.4% |
| </gallery> | | </gallery> |
|
| |
|
Line 208: |
Line 208: |
| File:C10184_11.jpg | | File:C10184_11.jpg |
| File:C10184_12.jpg | | File:C10184_12.jpg |
| File:Contour Plot Y33 EM_0_0 blue to red.jpg | | File:Contour Plot Y33 EM_0_0 blue to red.jpg| Uniformity: +-1.7% |
| </gallery> | | </gallery> |
Revision as of 12:54, 17 October 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
Start parameters, variations noted in the gallery headline
|
Recipe name: no 10 with lower platen power
|
Coil Power [W]
|
2500
|
Platen Power [W]
|
200
|
Platen temperature [oC]
|
20
|
H2 flow [sccm]
|
25.6
|
C4F8 flow [sccm]
|
25.6
|
He flow [sccm]
|
448.7
|
Pressure
|
Fully open APC valve (8-9 mTorr)
|
Electromagnetic coils (EM) 'outer coil' / 'inner coil'
|
'2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN)
|
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Results
Temporary conclusions on how the process parameters affect the results in this study:
|
What process parameters affect the results?
|
- Going from full wafer to small piece on Si carrier:
- Seemed to give more sidewall passivation
- Platen power: lowering the platen power gives
- more sidewall passivation
- lower etch rate
- Less trenching
- Removing the H2 gave:
- less sidewall passivation
- Adding O2 gave:
- less sidewall passivation
- Process pressure/total gasflow rate
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- less sidewall passivation
- Reduced the CD (Critical Dimensions)
- Coil power: Reducing coil power
- less CD loss
- more sidewall passivation
- Increasing process time:
- less sidewall passivation
- more sidewall bow
- CD loss due to larger mask faceting
|
- Sidewall passivation↑
- Sample size↓
- Platen power↓
- Coil power↓
- H2 flow↑
- O2 flow↓
- Total gas flow rate/pressure↑
|
- SiO2 etch with Cr mask on full wafer 6 min etch
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, O2:5sccm
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W
-
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT THIS LONG TIME), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W
-
-
-
-
-
-
-
Uniformity: +- 6.4%
- SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W
-
-
-
-
-
-
- SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch, EM:0/0 H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.9mTorr; platen power 100W, coil power:1200W
-
-
-
-
-
-
-
Uniformity: +-1.7%