Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions
No edit summary |
No edit summary |
||
Line 59: | Line 59: | ||
***Reduced the CD (Critical Dimensions) | ***Reduced the CD (Critical Dimensions) | ||
*Coil power: Reducing coil power | *Coil power: Reducing coil power | ||
**CD | **less CD loss | ||
**more sidewall passivation | **more sidewall passivation | ||
*Increasing process time: | *Increasing process time: |
Revision as of 13:01, 13 October 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
Start parameters, variations noted in the gallery headline | Recipe name: no 10 with lower platen power |
---|---|
Coil Power [W] | 2500 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
H2 flow [sccm] | 25.6 |
C4F8 flow [sccm] | 25.6 |
He flow [sccm] | 448.7 |
Pressure | Fully open APC valve (8-9 mTorr) |
Electromagnetic coils (EM) 'outer coil' / 'inner coil' | '2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN) |
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Results
Temporary conclusions on how the process parameters affect the results in this study
- Going from full wafer to small piece on Si carrier:
- Seemed to give more sidewall passivation
- Platen power: lowering the platen power gives
- more sidewall passivation
- lower etch rate
- Less trenching
- Removing the H2 gave:
- less sidewall passivation
- Adding O2 gave:
- less sidewall passivation
- Process pressure/total gasflow rate
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- less sidewall passivation
- Reduced the CD (Critical Dimensions)
- Reducing total gasflow rate which reduced the pressur inside the chamber gave:
- Coil power: Reducing coil power
- less CD loss
- more sidewall passivation
- Increasing process time:
- less sidewall passivation
- more sidewall bow
- CD loss due to larger mask faceting
-
pitch 800 nm
Top 461 nm
@edge 437 nm
bottom 402 nm
height 916 nm
height from edge 827 nm
Cr left 83.5 nm
selectivity 55.5 -
156 nm/min
-
pitch 800 nm
Top 444 nm
bottom 374 nm
height 718 nm
Cr left 85 nm
selectivity 48