Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions
No edit summary |
No edit summary |
||
Line 145: | Line 145: | ||
</gallery> | </gallery> | ||
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W" perrow="7" widths="200px" heights="150px"> | <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 14 min etch (PLEASE DO NOT REPEAT THIS LONG TIME), H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 100W, coil power:1200W" perrow="7" widths="200px" heights="150px"> | ||
File:C10160_02.jpg | File:C10160_02.jpg | ||
File:C10160_06.jpg | File:C10160_06.jpg | ||
Line 154: | Line 154: | ||
</gallery> | </gallery> | ||
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier | <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 10 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W" perrow="6" widths="200px" heights="150px"> | ||
File:C10161_01.jpg | File:C10161_01.jpg | ||
File:C10161_03.jpg | File:C10161_03.jpg |
Revision as of 11:23, 13 October 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
Start parameters, variations noted in the gallery headline | Recipe name: no 10 with lower platen power |
---|---|
Coil Power [W] | 2500 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
H2 flow [sccm] | 25.6 |
C4F8 flow [sccm] | 25.6 |
He flow [sccm] | 448.7 |
Pressure | Fully open APC valve (8-9 mTorr) |
Electromagnetic coils (EM) 'outer coil' / 'inner coil' | '2 A' / '30 A' |
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
-
pitch 800 nm
Top 461 nm
@edge 437 nm
bottom 402 nm
height 916 nm
height from edge 827 nm
Cr left 83.5 nm
selectivity 55.5
-
pitch 800 nm
Top 444 nm
bottom 374 nm
height 718 nm
Cr left 85 nm
selectivity 48