Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
Line 126: Line 126:
File:C10102_03__18.jpg
File:C10102_03__18.jpg
File:C10102_03__16.jpg
File:C10102_03__16.jpg
</gallery>
<gallery>
File:C10110_04.jpg
File:C10110_06.jpg
File:C10110_08.jpg
File:C10110_10.jpg
File:C10110_12.jpg
</gallery>
</gallery>

Revision as of 11:10, 9 October 2023

Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

Start parameters, variations noted in the gallery headline Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '2 A' / '30 A'
  • 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.