<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W" perrow="6" widths="200px" heights="150px"> | <gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W" perrow="6" widths="200px" heights="150px"> | ||
File:C10093_03__11.jpg | |||
File:C10093_03__09.jpg | File:C10093_03__09.jpg | ||
File:C10093_03__07.jpg | |||
File:C10093_03__05.jpg | |||
File:C10093_03__03.jpg | |||
File:C10093_03__01.jpg | File:C10093_03__01.jpg | ||
</gallery> | </gallery> |
Revision as of 15:50, 26 September 2023
Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
Start parameters, variations noted in the gallery headline | Recipe name: no 10 with lower platen power |
---|---|
Coil Power [W] | 2500 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
H2 flow [sccm] | 25.6 |
C4F8 flow [sccm] | 25.6 |
He flow [sccm] | 448.7 |
Pressure | Fully open APC valve (8-9 mTorr) |
Electromagnetic coils (EM) 'outer coil' / 'inner coil' | '2 A' / '30 A' |
- 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist and 65 nm barc.