Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

Start parameters, variations noted in the gallery headline Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '2 A' / '30 A'