Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
 
(8 intermediate revisions by the same user not shown)
Line 28: Line 28:
|}
|}


====Results when etching a ''non-patterned wafer''====
====Results with a ''non-patterned wafer''====


{| border="2" cellspacing="2" cellpadding="3"
{| border="2" cellspacing="2" cellpadding="3"
|-style="background:DarkGray; color:White"
|-style="background:DarkGray; color:White"
!Material to be etched
!Recipe
!Recipe: SIO2_ICP
!Recipe: SIO2_ICP
!SIO2_ICP on stoic Nit
!SIO2_ICP on stoic Nit
!SIO2_ICP on low-stress Nit
!SIO2_ICP on low-stress Nit
!SIO2_ICP on Si
|-
|-
|Etch rate in SiO2
|Etch rate
|155 nm/min in the center, 125nm/min in the edges
|121 nm/min  
(03052023 mfarin @ DTU nanolab)
(18.07.2023 mfarin @ DTU nanolab)
|194 nm/min  
|194 nm/min  
(24052023 mfarin @ DTU nanolab)
(24.05.2023 mfarin @ DTU nanolab)
|190 nm/min  
|190 nm/min  
(24052023 mfarin @ DTU nanolab)
(24.05.2023 mfarin @ DTU nanolab)
|
|-
|Etch rate in resist (AZ 5214E)
|108 nm/min in the center, 98nm/min in the edges
(03052023 mfarin @ DTU nanolab)
|
|
|
|-
|Selectivity (SiO2:resist)
|1.45
|
|
|
|-
|-


|Etch rate in silicon
|
|
|
|
|-
|Profile Images


|
|
|
|
|-
|}
|}


====Results when etching a patterned wafer ====
====Results with a ''patterned wafer'' ====


{| border="2" cellspacing="2" cellpadding="3"
{| border="2" cellspacing="2" cellpadding="3"
Line 89: Line 62:
|155 nm/min in the center, 125nm/min in the edges
|155 nm/min in the center, 125nm/min in the edges
(03052023 mfarin @ DTU nanolab)
(03052023 mfarin @ DTU nanolab)
|194 nm/min
|
(24052023 mfarin @ DTU nanolab)
|
|190 nm/min
(24052023 mfarin @ DTU nanolab)
|
|
|-
|-

Latest revision as of 15:25, 18 July 2023

Unless otherwise stated, all content in this section was done by Maria Farinha@DTU Nanolab, May 2023

This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.

Parameter Recipe name: SiO2_ICP
Coil Power [W] 1000
Platen Power [W] 200
Platen temperature [oC] 20
C4F8 flow [sccm] 10
H2 flow [sccm] 28
Pressure [mTorr] 2.5

Results with a non-patterned wafer

Recipe Recipe: SIO2_ICP SIO2_ICP on stoic Nit SIO2_ICP on low-stress Nit
Etch rate 121 nm/min

(18.07.2023 mfarin @ DTU nanolab)

194 nm/min

(24.05.2023 mfarin @ DTU nanolab)

190 nm/min

(24.05.2023 mfarin @ DTU nanolab)

Results with a patterned wafer

Material to be etched Recipe: SIO2_ICP SIO2_ICP on stoic Nit SIO2_ICP on low-stress Nit SIO2_ICP on Si
Etch rate in SiO2 155 nm/min in the center, 125nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Etch rate in resist (AZ 5214E) 108 nm/min in the center, 98nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Selectivity (SiO2:resist) 1.45
Etch rate in silicon
Profile Images SiO2 ICP.2-top-02.png

SiO2 ICP.2-top-04.png

  • More tests will be done regarding silicon and silicon nitride, since this recipe can be used for overetch.