Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/AlN deposition using ALD2: Difference between revisions

From LabAdviser
Tanamp (talk | contribs)
No edit summary
Pevo (talk | contribs)
No edit summary
 
(43 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/ALD2_(PEALD)/AlN_deposition_using_ALD2 click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/ALD2_(PEALD)/AlN_deposition_using_ALD2 click here]'''
 
''This page is written by DTU Nanolab internal''
 
 
=General Information=
=General Information=
The AlN process should never run above 350 °C due to the decomposition of the trimethylaluminium.
The AlN process should never run above 350 °C due to the decomposition of the trimethylaluminium.
As already mentioned in the general ALD2 (PEALD) page oxides and nitrides cannot be deposited at the same time. Since the aluminium nitride requires the plasma source we only run all nitride processes without the thermal lid.
As already mentioned in the general ALD2 (PEALD) page oxides and nitrides cannot be deposited at the same time. Since the aluminium nitride requires the plasma source, we run all plasma processes without the thermal lid. The substrate temperature is around 50 °C lower than the setpoint, because the chamber volume becomes bigger without the thermal lid.
Hence the chamber volume is bigger than with the thermal lid which causes that the substrate temperature is around 50 °C lower than the setpoint.


=Result from acceptance test=
=Results from the acceptance test=


==AlN with N<sub>2</sub> plasma== <!-- Experiment 161102A -->
During the acceptance test, AlN was deposited using TMA and N<sub>2</sub> plasma. We have modified and improved recipes since.
The test was done with 300 cycles at 350 &deg;C where the growth rate was measured to be '''0.0625 nm/cycle'''.  
* [[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/AlN deposition using ALD2/Acceptance_test_AlN|<b>results from the acceptance test (old material) </b>]].


=Deposition of AlN using TMA and NH3 plasma=
<b>Recipe name</b>: AlN NH3 plasma
<b>Temperature window</b>: 250 &deg;C - 350 &deg;C
The deposition rate is measure to be <b>0.137 nm/cycle</b> for 350 &deg;C with growth delay of 144 cycles.


{| border="2" cellspacing="2" cellpadding="5"  align="none"
{| border="2" cellspacing="2" cellpadding="5"  align="none"
Line 15: Line 25:
|
|
!TMA
!TMA
!N<sub>2</sub> plasma
!NH<sub>3</sub>
|-
|-
!Nitrogen flow
!Nitrogen flow
|100 sccm
|150 sccm
|150 sccm
|100 sccm
|-
|-
!Pulse time
!Pulse time
|0.1 s
|0.1 s
|21.0 s
|5 s
|-  
|-  
!Purge time
!Purge time
|4.0 s
|8 s
|4.0 s
|30 s
|-
|}
 
 
 
{| border="2" cellspacing="2" cellpadding="5"  align="center"
|-
!colspan="5" border="none" style="background:silver; color:black;" align="center"| Plasma source settings
|-
!RF power (W)
|<b>Ar carrier flow (sccm)</b>
|<b>Plasma gas flow (sccm)</b>
|<b>t<sub>1</sub> stabilization (s)</b>
|<b>t<sub>2</sub> RF Power on (s)</b>
 
|-
|3000
|150
|100
|1
|3.4
 
|-
|-
|}
|}
<gallery caption="" widths="500px" heights="500px" perrow="2">
 
image:AlN with N2 Ellipsometer.png
 
<b>Note!</b> Remember to obey the relation: [Pulse time - (t<sub>1</sub>+t<sub>2</sub>)] > 0.5 s
 
<gallery caption="" widths="500px" heights="400px" perrow="2">
image:eves_20200609_AlN_NH3_dep_rate.png| Deposition function for AlN with NH<sub>3</sub> plasma (350 &deg;C)
image:eves_20200609_AlN_NH3_SEM.png| Deposition of AlN with NH<sub>3</sub> plasma (500 cycles, 350 &deg;C) on si trench template. It is worth mention, that the process will not be good to passivate structures with an aspect ratio above 10.
</gallery>
 
<b>Evgeniy Shkondin, DTU Nanolab, 2020.</b>
 
==Spectroscopic ellipsometry==
 
The spectroscopic ellipsometry measurements were conducted by using [[Specific Process Knowledge/Characterization/Optical characterization|VASE Ellipsometer]]. The purpose of the investigation is to evaluate refractive index and dielectric function as well as to analyse the growth rate and uniformity.
 
 
===Refractive index and permittivity===
 
<gallery caption="" widths="500px" heights="400px" perrow="2">
image:eves_20200609_AlN_NH3_refractive_index.png| Refractive index and absorption koefficient as a function of wavelength.
image:eves_20200609_AlN_NH3_permittivity.png| Real and imaginary permittivity as a function of wavelength.
</gallery>
</gallery>
Uniformity profile across 150 mm Si wafer based on 49 measurement points measured with ellipsometer. The values for the grown oxide thickness can be seen in the table below.


===Thickness distribution and uniformity===
<gallery caption="" widths="500px" heights="400px" perrow="3">
image:eves_20200608_AlN_NH3_500cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 500cycles)
image:eves_20200608_AlN_NH3_568cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 568cycles)
image:eves_20200608_AlN_NH3_852cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 852cycles)
image:eves_20200608_AlN_NH3_1136cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 1136cycles)
image:eves_20200608_AlN_NH3_1704cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 1704cycles)
image:eves_20200608_AlN_NH3_2272cycles_SE_uniformity.png| Thickness distribution across the 100 mm wafer (350C 2272cycles)
</gallery>
{| border="2" cellspacing="2" cellpadding="5"  align="center"
|-
!colspan="7" border="none" style="background:silver; color:black;" align="center"| Ellipsometry results for AlN deposited with TMA and NH<sub>3</sub> plasma
|-
|<b>Number of cycles</b>
|<b>Temperature (&deg;C)</b>
|<b>Average thicknes (nm)</b>
|<b>Minimum thickness (nm)</b>
|<b>Maximum thickness (nm)</b>
|<b>Standard deviation</b>
|<b>Procent deviation (%)</b>
|-
|<b>500</b>
|350
|42.9565
|41.7422
|43.4888
|0.42652
|2.0331
|-
|<b>568</b>
|350
|66.1824
|64.2685
|67.4074
|0.7256
|2.3714
|-
|<b>852</b>
|350
|103.8306
|100.8147
|106.1143
|1.2407
|2.552
|-
|<b>1136</b>
|350
|128.1302
|124.8565
|131.037
|1.444
|2.4118
|-
|<b>1704</b>
|350
|203.6618
|198.1933
|210.8584
|2.7121
|3.1094


{| border="2" cellspacing="2" cellpadding="5"  align="none"
!Parameter
!Average
!Min.
!Max.
!Std.Dev
!%Range
|-
|-
!Thickness (nm)
|<b>2272</b>
|18.77
|350
|18.02
|298.1225
|19.73
|293.8553
|0.41
|305.0185
|9.0619
|2.3923
|1.8723
 
|}
|}


<b>Pernille Voss Larsen, Mikkel Dysseholm Mar and Tanja Amport, DTU Danchip, 2016-2017.</b>


==AlN with N<sub>2</sub> plasma on trenches== <!-- Experiment 161102B and 161104A -->
<b>Evgeniy Shkondin, DTU Nanolab, 2020.</b>
The test was done with 1000 cycles at 350 &deg;C.


==X-ray photoelectron spectroscopy==
XPS measurements of all samples has been performed using [[Specific Process Knowledge/Characterization/XPS/K-Alpha |XPS K-Alpha equipment]]. The purpose of the investigation is to get idea about film stoichiometry and possible contamination.
===Stoichiometry===
{| border="2" cellspacing="2" cellpadding="5"  align="center"


{| border="2" cellspacing="2" cellpadding="5"  align="none"
|-  
|-  
|
!colspan="6" border="none" style="background:silver; color:black;" align="center"| Stoichiometry results for AlN deposited with TMA and NH<sub>3</sub> plasma
!TMA
|-
!N<sub>2</sub> plasma
|style="background:WhiteSmoke; color:black"|<b>Number of cycles</b>
|style="background:WhiteSmoke; color:black"|<b>568</b>
|style="background:WhiteSmoke; color:black"|<b>852</b>
|style="background:WhiteSmoke; color:black"|<b>1136</b>
|style="background:WhiteSmoke; color:black"|<b>1704</b>
|style="background:WhiteSmoke; color:black"|<b>2272</b>
 
|-
|style="background:WhiteSmoke; color:black"|<b>Average thickness (nm)</b>
|style="background:WhiteSmoke; color:black"|66.18
|style="background:WhiteSmoke; color:black"|103.83
|style="background:WhiteSmoke; color:black"|128.13
|style="background:WhiteSmoke; color:black"|203.66
|style="background:WhiteSmoke; color:black"|298.12
 
|-
|-
!Nitrogen flow
|<b>Al (at.%)</b>
|150 sccm
|47.54
|100 sccm
|48.15
|47.82
|47.77
|47.61
 
|-
|-
!Pulse time
|<b>N (at.%)</b>
|0.1 s
|40.80
|26.0 s
|40.60
|-
|41.13
!Purge time
|41.01
|4.0 s
|41.11
|15.0 s
 
|-
|-
|<b>O (at.%)</b>
|11.66
|11.25
|11.05
|11.22
|11.28
|}
|}
Additionally the picoflow was used for the TMA precursor.
 
<gallery caption="" widths="500px" heights="500px" perrow="2">
===Presence of Oxygen and Carbon===
image:AlN with N2 trenches2 SEM.png
 
image:AlN with N2 trenches SEM.png
Traces of carbon is found in the deposited films, their origine is not clear, but most likely due to TMA decomposition. Another source is incomplete ALD reaction.
image:AlN with N2 trenches3 SEM.png
Oxygen is present in the film (up to 11 at.%)
 
<gallery caption="" widths="500px" heights="400px" perrow="2">
image:eves_20200609_AlN_NH3_XPS_C1s.png| C1s signal
image:eves_20200609_AlN_NH3_XPS_O1s.png| O1s signal
</gallery>
</gallery>
As the SEM images above show only a thin layer of AlN could be deposited at the bottom of the trenches. On the top the growth was significantly higher which lead to a tree like growth.
<gallery caption="" widths="500px" heights="350px" perrow="2">
Whereas in the images below no picoflow was used with 500 cycles and the same other parameters as in the run shown above. Without the picoflow a more homogeneous coverage could be obtained and an average growth rate of '''0,05585 nm/cycle''' was measured. 
image:eves_20200609_AlN_NH3_XPS_3D_C1s.png| C1s signal
<gallery caption="" widths="500px" heights="500px" perrow="2">
image:eves_20200609_AlN_NH3_XPS_3D_O1s.png| O1s signal
image:AlN 00.png
image:AlN bottom 03.png
image:AlN top 01.png
</gallery>
</gallery>


 
<b>Evgeniy Shkondin, DTU Nanolab, 2020.</b>
<b>Pernille Voss Larsen, Mikkel Dysseholm Mar and Tanja Amport, DTU Danchip, 2016-2017.</b>

Latest revision as of 13:10, 19 June 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal


General Information

The AlN process should never run above 350 °C due to the decomposition of the trimethylaluminium. As already mentioned in the general ALD2 (PEALD) page oxides and nitrides cannot be deposited at the same time. Since the aluminium nitride requires the plasma source, we run all plasma processes without the thermal lid. The substrate temperature is around 50 °C lower than the setpoint, because the chamber volume becomes bigger without the thermal lid.

Results from the acceptance test

During the acceptance test, AlN was deposited using TMA and N2 plasma. We have modified and improved recipes since.

Deposition of AlN using TMA and NH3 plasma

Recipe name: AlN NH3 plasma

Temperature window: 250 °C - 350 °C

The deposition rate is measure to be 0.137 nm/cycle for 350 °C with growth delay of 144 cycles.

TMA NH3
Nitrogen flow 100 sccm 150 sccm
Pulse time 0.1 s 5 s
Purge time 8 s 30 s


Plasma source settings
RF power (W) Ar carrier flow (sccm) Plasma gas flow (sccm) t1 stabilization (s) t2 RF Power on (s)
3000 150 100 1 3.4


Note! Remember to obey the relation: [Pulse time - (t1+t2)] > 0.5 s

Evgeniy Shkondin, DTU Nanolab, 2020.

Spectroscopic ellipsometry

The spectroscopic ellipsometry measurements were conducted by using VASE Ellipsometer. The purpose of the investigation is to evaluate refractive index and dielectric function as well as to analyse the growth rate and uniformity.


Refractive index and permittivity

Thickness distribution and uniformity


Ellipsometry results for AlN deposited with TMA and NH3 plasma
Number of cycles Temperature (°C) Average thicknes (nm) Minimum thickness (nm) Maximum thickness (nm) Standard deviation Procent deviation (%)
500 350 42.9565 41.7422 43.4888 0.42652 2.0331
568 350 66.1824 64.2685 67.4074 0.7256 2.3714
852 350 103.8306 100.8147 106.1143 1.2407 2.552
1136 350 128.1302 124.8565 131.037 1.444 2.4118
1704 350 203.6618 198.1933 210.8584 2.7121 3.1094
2272 350 298.1225 293.8553 305.0185 2.3923 1.8723


Evgeniy Shkondin, DTU Nanolab, 2020.

X-ray photoelectron spectroscopy

XPS measurements of all samples has been performed using XPS K-Alpha equipment. The purpose of the investigation is to get idea about film stoichiometry and possible contamination.

Stoichiometry

Stoichiometry results for AlN deposited with TMA and NH3 plasma
Number of cycles 568 852 1136 1704 2272
Average thickness (nm) 66.18 103.83 128.13 203.66 298.12
Al (at.%) 47.54 48.15 47.82 47.77 47.61
N (at.%) 40.80 40.60 41.13 41.01 41.11
O (at.%) 11.66 11.25 11.05 11.22 11.28

Presence of Oxygen and Carbon

Traces of carbon is found in the deposited films, their origine is not clear, but most likely due to TMA decomposition. Another source is incomplete ALD reaction. Oxygen is present in the film (up to 11 at.%)

Evgeniy Shkondin, DTU Nanolab, 2020.