Specific Process Knowledge/Thin Film deposition/ALD/Al2O3 deposition using ALD: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Pevo (talk | contribs)
No edit summary
 
(2 intermediate revisions by 2 users not shown)
Line 2: Line 2:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_Film_deposition/ALD/Al2O3_deposition_using_ALD click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_Film_deposition/ALD/Al2O3_deposition_using_ALD click here]'''


''This page is written by DTU Nanolab internal''


The ALD window for depostion of aluminium dioxide (Al<sub>2</sub>O<sub>3</sub>) ranges from 150 <sup>o</sup>C to 350 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 350 <sup>o</sup>C the TMA decomposes.


All results shown on this page have been obtained using the "AL2O3" recipe on new Si(100) wafers with native oxide:
The ALD window for depostion of aluminium oxide (Al<sub>2</sub>O<sub>3</sub>) ranges from 150 <sup>o</sup>C to 300 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 300 <sup>o</sup>C the TMA decomposes.
 
All results shown on this page have been obtained by depositing Al2O3 on new Si(100) wafers with native oxide using the "AL2O3" recipe.
 


====Al<sub>2</sub>O<sub>3</sub> standard recipe====
====Al<sub>2</sub>O<sub>3</sub> standard recipe====
Line 43: Line 46:
|}
|}


In the graphs below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickness can be calculated.


In the graphs below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. The points have been fitted to a linear curve, and the slope of this curve shows the deposition rate. So from the equation the number of cycles required for a certain thickness of Al<sub>2</sub>O<sub>3</sub> to be deposited can be calculated.


<gallery caption="Aluminium oxide thickness as function of number of cycles" widths="250px" heights="250px" perrow="5">
<gallery caption="Aluminium oxide thickness as function of number of cycles" widths="250px" heights="250px" perrow="5">
Line 54: Line 57:
</gallery>
</gallery>


Evgeniy Shkondin, DTU Danchip, February-March 2014.
Evgeniy Shkondin, DTU Nanolab, February-March 2014.

Latest revision as of 10:26, 19 June 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal


The ALD window for depostion of aluminium oxide (Al2O3) ranges from 150 oC to 300 oC. XPS measurements shows that at temperatures below 150 oC the Al2O3 layer will be contaminated by unreacted TMA molecules, and at temperatures above 300 oC the TMA decomposes.

All results shown on this page have been obtained by depositing Al2O3 on new Si(100) wafers with native oxide using the "AL2O3" recipe.


Al2O3 standard recipe

Recipe: AL2O3

Temperature: 150 oC - 350 oC

TMA H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.1 s
Purge time 3.0 s 4.0 s


Al2O3 deposition rates

The deposition rate for Al2O3 depends on the temperature, see the graph below.

Al2O3 deposition rate as function of temperature.


In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. The points have been fitted to a linear curve, and the slope of this curve shows the deposition rate. So from the equation the number of cycles required for a certain thickness of Al2O3 to be deposited can be calculated.

Evgeniy Shkondin, DTU Nanolab, February-March 2014.