The ALD window for depostion of aluminium oxide (Al<sub>2</sub>O<sub>3</sub>) ranges from 150 <sup>o</sup>C to 300 <sup>o</sup>C. XPS measurements shows that at temperatures below 150 <sup>o</sup>C the Al<sub>2</sub>O<sub>3</sub> layer will be contaminated by unreacted TMA molecules, and at temperatures above 300 <sup>o</sup>C the TMA decomposes. | |||
All results shown on this page have been obtained by depositing Al2O3 on new Si(100) wafers with native oxide using the "AL2O3" recipe. | |||
====Al<sub>2</sub>O<sub>3</sub> standard recipe==== | |||
<b>Recipe</b>: AL2O3 | <b>Recipe</b>: AL2O3 | ||
Line 32: | Line 36: | ||
|} | |} | ||
====Al<sub>2</sub>O<sub>3</sub> deposition rates==== | |||
The deposition rate for Al<sub>2</sub>O<sub>3</sub> depends on the temperature, see the graph below. | The deposition rate for Al<sub>2</sub>O<sub>3</sub> depends on the temperature, see the graph below. | ||
Line 41: | Line 47: | ||
In the graphs below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. | In the graphs below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 150 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. The points have been fitted to a linear curve, and the slope of this curve shows the deposition rate. So from the equation the number of cycles required for a certain thickness of Al<sub>2</sub>O<sub>3</sub> to be deposited can be calculated. | ||
<gallery caption="Aluminium oxide thickness as function of number of cycles" widths="250px" heights="250px" perrow="5"> | <gallery caption="Aluminium oxide thickness as function of number of cycles" widths="250px" heights="250px" perrow="5"> | ||
Line 51: | Line 57: | ||
</gallery> | </gallery> | ||
Evgeniy Shkondin, DTU Nanolab, February-March 2014. | |||
Evgeniy Shkondin, DTU |
Latest revision as of 10:26, 19 June 2023
Feedback to this page: click here
This page is written by DTU Nanolab internal
The ALD window for depostion of aluminium oxide (Al2O3) ranges from 150 oC to 300 oC. XPS measurements shows that at temperatures below 150 oC the Al2O3 layer will be contaminated by unreacted TMA molecules, and at temperatures above 300 oC the TMA decomposes.
All results shown on this page have been obtained by depositing Al2O3 on new Si(100) wafers with native oxide using the "AL2O3" recipe.
Al2O3 standard recipe
Recipe: AL2O3
Temperature: 150 oC - 350 oC
TMA | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 3.0 s | 4.0 s |
Al2O3 deposition rates
The deposition rate for Al2O3 depends on the temperature, see the graph below.
In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. The points have been fitted to a linear curve, and the slope of this curve shows the deposition rate. So from the equation the number of cycles required for a certain thickness of Al2O3 to be deposited can be calculated.
-
Temperature 150 oC.
-
Temperature 200 oC.
-
Temperature 250 oC.
-
Temperature 300 oC.
-
Temperature 350 oC.