Specific Process Knowledge/Thin film deposition/Deposition of Hafnium Oxide: Difference between revisions
No edit summary |
|||
(4 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Hafnium_Oxide click here]''' | ||
<!-- Replace "http://labadviser.danchip.dtu.dk/..." wih the link to the Labadviser page--> | <!-- Replace "http://labadviser.danchip.dtu.dk/..." wih the link to the Labadviser page--> | ||
''All contents by Nanolab staff.'' | |||
<br clear="all" /> | <br clear="all" /> | ||
Line 7: | Line 9: | ||
Thin films of hafnium oxide, HfO<sub>2</sub>, can both be deposited both in the [[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD1]] and the [[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)|ALD2 (PEALD)]]. However, it is preferred to use the ALD1, as the ALD2 is mainly dedicated for nitride deposition. | Thin films of hafnium oxide, HfO<sub>2</sub>, can both be deposited both in the [[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD1]] and the [[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)|ALD2 (PEALD)]]. However, it is preferred to use the ALD1, as the ALD2 is mainly dedicated for nitride deposition. | ||
More information about hafnium oxide deposition can be found here: for [[ | More information about hafnium oxide deposition can be found here: for [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/HfO2_deposition_using_ALD_new_page|ALD1]] and for [[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/HfO2 deposition using ALD2|ALD2 (PEALD)]]. | ||
== | ==Deposition of hafnium oxide== | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
Line 16: | Line 18: | ||
|- | |- | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
| | |||
![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD1]] | |||
![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200| | ![[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)|ALD2 (PEALD)]]. | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
Line 24: | Line 26: | ||
| | | | ||
*Atomic Layer Deposition | *Atomic Layer Deposition | ||
| | |||
*(Plasma enhanced) Atomic Layer Deposition | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Stoichiometry | !Stoichiometry | ||
| | | | ||
* | *HfO<sub>2</sub> | ||
| | |||
*HfO<sub>2</sub> | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Film Thickness | !Film Thickness | ||
| | | | ||
* 0 nm - 50 nm | *0 nm - 100 nm | ||
| | |||
*0 nm - 50 nm | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Deposition rate | !Deposition rate | ||
| | | | ||
* 0.0827 nm/cycle | * At 150 <sup>o</sup>C: 0.11 nm/cycle | ||
* 0.954- | * At 250 <sup>o</sup>C: 0.0827 nm/cycle | ||
| | |||
* At 250 <sup>o</sup>C: 0.0804 nm/cycle | |||
* At 250 <sup>o</sup>C on trenches: 0.954-1.22 nm/cycle | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Step coverage | !Step coverage | ||
| | |||
*Very good. | |||
| | | | ||
*Very good | *Very good | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! | !Temperature window | ||
| | |||
*150 <sup>o</sup>C - 300 <sup>o</sup>C | |||
| | | | ||
* 150 - 300<sup>o</sup>C | *150 <sup>o</sup>C - 300 <sup>o</sup>C | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Substrate size | !Substrate size | ||
| | | | ||
*1-5 100 mm wafers (only good uniformity for the top wafer) | |||
*1-5 | *1-5 150 mm wafer (only good uniformity for the top wafer) | ||
*1-5 100 mm | *1 200 mm wafer | ||
*1 | *Several smaller samples | ||
| | |||
*1 100 mm wafer | |||
*1 150 mm wafer | |||
*1 200 mm wafer | |||
*Several smaller samples | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
Line 65: | Line 85: | ||
*Silicon oxide, silicon nitride | *Silicon oxide, silicon nitride | ||
*Quartz/fused silica | *Quartz/fused silica | ||
* | *Metals (use dedicated carrier wafer) | ||
* | *III-V materials (use dedicated carrier wafer) | ||
* | *Polymers (depending on the melting point/deposition temperature, use carrier wafer) | ||
| | |||
*Silicon | |||
*Silicon oxide, silicon nitride | |||
*Quartz/fused silica | |||
*Metals (use dedicated carrier wafer) | |||
*III-V materials (use dedicated carrier wafer) | *III-V materials (use dedicated carrier wafer) | ||
*Polymers (depending on the melting point/deposition temperature, use carrier wafer) | *Polymers (depending on the melting point/deposition temperature, use carrier wafer) | ||
|- | |- | ||
|} | |} |
Latest revision as of 11:35, 9 June 2023
Feedback to this page: click here
All contents by Nanolab staff.
Deposition of Hafnium Oxide
Thin films of hafnium oxide, HfO2, can both be deposited both in the ALD1 and the ALD2 (PEALD). However, it is preferred to use the ALD1, as the ALD2 is mainly dedicated for nitride deposition.
More information about hafnium oxide deposition can be found here: for ALD1 and for ALD2 (PEALD).
Deposition of hafnium oxide
ALD1 | ALD2 (PEALD). | |
---|---|---|
Generel description |
|
|
Stoichiometry |
|
|
Film Thickness |
|
|
Deposition rate |
|
|
Step coverage |
|
|
Temperature window |
|
|
Substrate size |
|
|
Allowed materials |
|
|