Specific Process Knowledge/Thin film deposition/Deposition of Nickel: Difference between revisions
Line 6: | Line 6: | ||
== Nickel deposition == | == Nickel deposition == | ||
Nickel can be deposited by e-beam evaporation | Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering. | ||
*[[/Electroplating of nickel|Electroplating of nickel]] | Some process information is available here for e-beam evaporated films: | ||
<!--*[[/Electroplating of nickel|Electroplating of nickel]]--> | |||
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | *[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | ||
In the chart below you can compare the different deposition equipment: | |||
{| border="1" cellspacing="0" cellpadding="3" | {| border="1" cellspacing="0" cellpadding="3" | ||
Line 20: | Line 21: | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ||
|- | |- | ||
Line 30: | Line 30: | ||
|Sputter deposition of Nickel | |Sputter deposition of Nickel | ||
|Sputter deposition of Nickel | |Sputter deposition of Nickel | ||
|- | |- | ||
Line 40: | Line 39: | ||
|RF Ar clean | |RF Ar clean | ||
|RF Ar clean | |RF Ar clean | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
Line 49: | Line 47: | ||
|10 Å to 5000 Å ** | |10 Å to 5000 Å ** | ||
|10 Å to 5000 Å ** | |10 Å to 5000 Å ** | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
Line 58: | Line 55: | ||
|Depends on process parameters, about 1 Å/s | |Depends on process parameters, about 1 Å/s | ||
|Depends on process parameters, at least ~ 4 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]] | |Depends on process parameters, at least ~ 4 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]] | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
Line 78: | Line 74: | ||
*Up to 10x4" or 6" wafers | *Up to 10x4" or 6" wafers | ||
*Many smaller pieces | *Many smaller pieces | ||
|- | |- | ||
Line 110: | Line 102: | ||
| | | | ||
*Almost any that do not outgas. Check the cross-contamination sheet in Labmanager. | *Almost any that do not outgas. Check the cross-contamination sheet in Labmanager. | ||
|- | |- | ||
|- | |- | ||
Line 133: | Line 114: | ||
| | | | ||
*May use high-strength magnet for deposition | *May use high-strength magnet for deposition | ||
|- | |- | ||
Revision as of 10:45, 9 June 2023
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Labmanager Including APV and QC requires login.
Nickel deposition
Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.
Some process information is available here for e-beam evaporated films:
In the chart below you can compare the different deposition equipment:
E-beam evaporation (Temescal) | E-beam evaporation (Wordentec) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
---|---|---|---|---|
General description | E-beam deposition of Nickel | E-beam deposition of Nickel | Sputter deposition of Nickel | Sputter deposition of Nickel |
Pre-clean | Ar ion bombardment | RF Ar clean | RF Ar clean | |
Layer thickness | 10 Å to 1 µm * | 10 Å to 1 µm * | 10 Å to 5000 Å ** | 10 Å to 5000 Å ** |
Deposition rate | 2-10 Å/s | 10-15 Å/s | Depends on process parameters, about 1 Å/s | Depends on process parameters, at least ~ 4 Å/s, see conditions here |
Batch size |
|
|
|
|
Allowed materials |
|
|
|
|
Comment |
|
|
* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
Quality control of e-beam evaporated Ni films
Quality control (QC) for Wordentec | ||||||||||||||||
Thickness is measured in 5 points with a stylus profiler. |
Quality control (QC) for the Temescal | ||||||||||||||||||
Thickness is measured in 5 points with a stylus profiler. |