Specific Process Knowledge/Thin film deposition/Deposition of Chromium/Sputtering of Cr in Wordentec: Difference between revisions
Created page with "'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/Specific_Process_Knowledge/Thin_film_dep..." |
No edit summary |
||
(5 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Chromium/Sputtering_of_Cr_in_Wordentec click here]''' | ||
''All text by DTU Nanolab staff'' | |||
== Deposition rate == | == Deposition rate == | ||
Depending on the settings (pressure and power) during the sputtering process, '''the uniformity and grain size of the deposited layer will be different''' (see study on[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Chromium/Deposition_of_Chromium| Uniformity of sputtered chromium]]) | |||
The deposition rate will also change with the settings. | The deposition rate will also change with the settings. | ||
The following data is from the [[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]] | |||
'''Pressure <math>1*10^{-3}</math> mbar, | '''Pressure <math>1*10^{-3}</math> mbar, power 150 W''' | ||
The rate is established to be 1.1 Å/s (in the center of the wafer, 1.0 Å/s at the edge). | The rate is established to be 1.1 Å/s (in the center of the wafer, 1.0 Å/s at the edge). | ||
Line 17: | Line 19: | ||
'''Pressure <math>4*10^{-3}</math> mbar, | '''Pressure <math>4*10^{-3}</math> mbar, power 300 W''' | ||
The rate is established to be 2.3 Å/s (in the center of the wafer, 2.0 Å/s at the edge). | The rate is established to be 2.3 Å/s (in the center of the wafer, 2.0 Å/s at the edge). | ||
This corresponds to a deposition time of '''44 seconds''' for deposition of '''10 nm'''. | This corresponds to a deposition time of '''44 seconds''' for deposition of '''10 nm'''. |
Latest revision as of 15:54, 6 June 2023
Feedback to this page: click here
All text by DTU Nanolab staff
Deposition rate
Depending on the settings (pressure and power) during the sputtering process, the uniformity and grain size of the deposited layer will be different (see study on Uniformity of sputtered chromium)
The deposition rate will also change with the settings.
The following data is from the Wordentec
Pressure mbar, power 150 W
The rate is established to be 1.1 Å/s (in the center of the wafer, 1.0 Å/s at the edge).
This corresponds to a deposition time of 1 minute 34 seconds for deposition of 10 nm.
Pressure mbar, power 300 W
The rate is established to be 2.3 Å/s (in the center of the wafer, 2.0 Å/s at the edge).
This corresponds to a deposition time of 44 seconds for deposition of 10 nm.