Specific Process Knowledge/Thin film deposition/Deposition of Aluminium Nitride: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
(15 intermediate revisions by 5 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium_Nitride click here]''' | ||
''All text by DTU Nanolab staff'' | |||
<br clear="all" /> | <br clear="all" /> | ||
Line 6: | Line 7: | ||
== Deposition of Aluminium Nitride == | == Deposition of Aluminium Nitride == | ||
AlN can be deposited by | AlN films can be deposited by sputtering or by atomic layer deposition (ALD). | ||
In the sputter systems AlN can be either deposited by direct sputtering of an AlN target or reactive sputtering with an Al target in mixtures of argon and nitrogen. | |||
== | ==Comparison of the methods for deposition of AlN== | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
Line 22: | Line 20: | ||
! | ! | ||
![[Specific Process Knowledge/Thin film deposition/ | ![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System (Lesker)]] | ||
![[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Nitride(PC3)]] | |||
![[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)|ALD2]] | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
| | | | ||
*Reactive Sputtering (Al target) | *Reactive Sputtering (2" Al target) | ||
| | |||
*Pulsed reactive DC sputtering (PDC, 4" Al target) | |||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | |||
| | |||
*Plasma Enhanced Atomic Layer Deposition | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Stoichiometry | !Stoichiometry | ||
| | | | ||
* | *Oxygen contamination issue (in 2016 a user got ~ 30 % O in the AlN, measured by XPS in the bulk of the layer). | ||
| | |||
*Al:N:O ~ 53 : 46 : 1.5 in the bulk (see acceptance test results [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Process information|here]]). It should be possible to tune the Al:N ratio somewhat. | |||
| | |||
*AlN | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Film Thickness | !Film Thickness | ||
| | | | ||
* 0nm - | * few nm - 200 nm | ||
| | |||
* few nm - ~ 1 μm | |||
| | |||
* 0nm - 50 nm | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Deposition rate | !Deposition rate | ||
| | | | ||
* | * 0.055 nm/s (Power: 300W, pressure:1 mTorr, temp.: 400C, N2 ratio: 50%) | ||
| | |||
* at least 0.5 nm/s ([[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard recipe performance|see conditions]]) | |||
| | |||
* 0.0625 nm/cycle on a flat sample | |||
* 0.0558 nm/cycle on a high aspect ratio structures | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Step coverage | !Step coverage | ||
| | |||
*Good | |||
| | |||
*Not known, most likely medium-good | |||
| | | | ||
*Very good | *Very good | ||
Line 52: | Line 74: | ||
!Process Temperature | !Process Temperature | ||
| | | | ||
* Up to 400 | * Up to 400 °C | ||
| | |||
* Up to 600 °C | |||
| | |||
* 350 °C | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Substrate size | !Substrate size | ||
| | | | ||
* 100 mm wafers | * chips | ||
* 150 mm | * 1x 100 mm wafer | ||
* 1x 150 mm wafer | |||
| | |||
* chips | |||
* 10 x 100 mm wafer or | |||
* 10 x 150 mm wafer | |||
| | |||
*Several small samples | |||
*1 50 mm wafers | |||
*1 100 mm wafers | |||
*1 150 mm wafer | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! | !Allowed materials | ||
| | | | ||
Line 72: | Line 108: | ||
*SU-8 | *SU-8 | ||
*Any metals | *Any metals | ||
| | |||
*Similar to the Sputter-System (Lesker), see [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 cross-contamination sheet] | |||
| | |||
*Silicon | |||
*Silicon oxide, silicon nitride | |||
*Quartz/fused silica | |||
*Al, Al<sub>2</sub>O<sub>3</sub> | |||
*Ti, TiO<sub>2</sub> | |||
*Other metals (use dedicated carrier wafer) | |||
*III-V materials (use dedicated carrier wafer) | |||
*Polymers (depending on the melting point/deposition temperature, use carrier wafer) | |||
|- | |- | ||
|} | |} | ||
Further process information can be found here: | |||
*[[Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/AlN deposition using ALD2|AlN deposition using ALD2]] | |||
*[[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Process information|Deposition conditions and acceptance test results]] for sputter deposition of AlN in the Sputter-System Metal-Nitride(PC3). | |||
*For further information on AlN deposition using the sputter systems please contact the Thin Film Group ([mailto:thinfilm@nanolab.dtu.dk thinfilm@nanolab.dtu.dk]). The Sputter-System Metal-Nitride(PC3) was acquired partly to make it possible to deposit high-quality of AlN films. |
Latest revision as of 15:41, 1 June 2023
Feedback to this page: click here
All text by DTU Nanolab staff
Deposition of Aluminium Nitride
AlN films can be deposited by sputtering or by atomic layer deposition (ALD).
In the sputter systems AlN can be either deposited by direct sputtering of an AlN target or reactive sputtering with an Al target in mixtures of argon and nitrogen.
Comparison of the methods for deposition of AlN
Sputter-System (Lesker) | Sputter-System Metal-Nitride(PC3) | ALD2 | |
---|---|---|---|
Generel description |
|
|
|
Stoichiometry |
|
|
|
Film Thickness |
|
|
|
Deposition rate |
|
|
|
Step coverage |
|
|
|
Process Temperature |
|
|
|
Substrate size |
|
|
|
Allowed materials |
|
|
|
Further process information can be found here:
- AlN deposition using ALD2
- Deposition conditions and acceptance test results for sputter deposition of AlN in the Sputter-System Metal-Nitride(PC3).