'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/IBSD_of_SiO2 click here]''' <br> | ||
{{CC1}} | |||
Line 6: | Line 6: | ||
==Acceptance test for SiO2 deposition (2011) on IBE/IBSD Ionfab 300+)== | |||
{| border="2" cellspacing="0" cellpadding="2" | {| border="2" cellspacing="0" cellpadding="2" | ||
|- | |- | ||
Line 20: | Line 20: | ||
*50 mm SSP Si wafer | *50 mm SSP Si wafer | ||
*525 µm thick | *525 µm thick | ||
*Supplied by | *Supplied by Nanolab | ||
| | | | ||
*100 mm SSP Si wafer | *100 mm SSP Si wafer | ||
Line 32: | Line 32: | ||
*SiO2 | *SiO2 | ||
The purpose of the SiO2 is to be part of a mirror: <br\> | The purpose of the SiO2 is to be part of a mirror: <br\> | ||
5 | 5 quarter wavelength pairs of <br\> | ||
SiO2 <br\> | SiO2 <br\> | ||
TiO2 <br\> | TiO2 <br\> | ||
Extra | Extra quarter wavelength layer of <br\> | ||
TiO2 <br\> | TiO2 <br\> | ||
5 | 5 quarter wavelength pairs of <br\> | ||
SiO2 <br\> | SiO2 <br\> | ||
TiO2 <br\> | TiO2 <br\> | ||
Line 50: | Line 50: | ||
!style="background:silver; color:black" align="left" valign="top"|Deposition thickness | !style="background:silver; color:black" align="left" valign="top"|Deposition thickness | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *222 nm | ||
| | | | ||
*~ | *~215 nm | ||
| | | | ||
*224nm | *224nm | ||
Line 60: | Line 60: | ||
*6 nm/min | *6 nm/min | ||
| | | | ||
*7. | *7.42 nm/min +- 0.04nm/min | ||
One standard deviation | One standard deviation | ||
| | | | ||
*7. | *7.73 nm/min | ||
Only made once | Only made once | ||
|- | |- | ||
Line 84: | Line 84: | ||
!style="background:silver; color:black" align="left" valign="top"|Stress | !style="background:silver; color:black" align="left" valign="top"|Stress | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*< | *<500 MPa | ||
| | | | ||
*~ | *~600 MPa | ||
| | | | ||
* | *475 MPa | ||
|- | |- | ||
!style="background:silver; color:black" align="left" valign="top"|Refractive index | !style="background:silver; color:black" align="left" valign="top"|Refractive index | ||
Line 110: | Line 110: | ||
|- | |- | ||
|Platen rotation speed | |Platen rotation speed | ||
| | |20 rpm | ||
| | |20 rpm | ||
|- | |- | ||
|Ar(N) flow | |Ar(N) flow | ||
Line 122: | Line 122: | ||
|- | |- | ||
|I(N) | |I(N) | ||
| | |310 mA | ||
| | |320 mA | ||
|- | |- | ||
|Power | |Power | ||
| | |675 W | ||
| | |700 W | ||
|- | |- | ||
|I(B) | |I(B) | ||
| | |310 mA | ||
| | |280 mA | ||
|- | |- | ||
|V(B) | |V(B) | ||
| | |1200 V | ||
| | |1100 V | ||
|- | |- | ||
|Vacc(B) | |Vacc(B) | ||
| | |400 V | ||
| | |400 V | ||
|- | |- | ||
|Deposition time | |Deposition time | ||
| | |29 min | ||
| | |37 min | ||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
==Other results== | ==Other results== | ||
===Roughness of the surface=== | ===Roughness of the surface=== | ||
Measured with the Optical profiler - PSI mode (on one sample from the | Measured with the Optical profiler - PSI mode (on one sample from the acceptance test): Sa= 0.6 nm | ||
===Uniformity and break down voltage ''by Mathias Engholm 2016-11-29''=== | ===Uniformity and break down voltage ''by Mathias Engholm 2016-11-29''=== | ||
Mathias made 105.62nm SiO2 on a test silicon wafer and on his sample wafer. The sample wafer had gold/Cr on the surface and that had to be electrically isolated. The uniformity over the wafer of the oxide was 0.19% over 9 points - this is better than he has achieved when oxidizing in a furnace. He anodic bonded the wafer without problems. He measured the breakdown voltage and got 0.82+/+ 0.13 V/nm over 24 points. This is just as good as the oxide from the furnaces. Before his deposition he ran a | Mathias made 105.62nm SiO2 on a test silicon wafer and on his sample wafer. The sample wafer had gold/Cr on the surface and that had to be electrically isolated. The uniformity over the wafer of the oxide was 0.19% over 9 points - this is better than he has achieved when oxidizing in a furnace. He anodic bonded the wafer without problems. He measured the breakdown voltage and got 0.82+/+ 0.13 V/nm over 24 points. This is just as good as the oxide from the furnaces. Before his deposition he ran a 20 min heat up and 40min dummy deposition to clean the target. This was done with a bright new target and with the small deposition grids mounted.<br> | ||
[[File:breakdownvoltage.png|400px]] | [[File:breakdownvoltage.png|thumb|left|400px| Breakdown voltage over the wafer, ''by Mathias Engholm 2016-11-29'']] | ||
[[ | [[File:Ibsd uniformity SiO2.jpg|thumb|none|500px| Thickness uniformity over the wafer, ''by Mathias Engholm 2016-11-29'']]<br> |
Latest revision as of 11:56, 24 March 2023
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Go to 'IBE/IBSD Ionfab 300' equipment page
Acceptance test for SiO2 deposition (2011) on IBE/IBSD Ionfab 300+)
. | Acceptance Criteria |
Acceptance Result 1 |
Acceptance Result 2 |
---|---|---|---|
Substrate information |
|
|
|
Material to be deposited |
The purpose of the SiO2 is to be part of a mirror: <br\> 5 quarter wavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Extra quarter wavelength layer of <br\> TiO2 <br\> 5 quarter wavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Design wavelength (for refractive indices and layer thicknesses): 1300nm <br\> The acceptance criteria is set up for the single SiO2 and TiO2 layers. <br\> Five runs in a row for each material. |
|
|
Deposition thickness |
|
|
|
Deposition rate |
|
One standard deviation |
Only made once |
Thickness uniformity |
|
|
|
Reproducibility |
|
|
|
Stress |
|
|
|
Refractive index | . |
|
|
Recipe 1 | Recipe 2 | |
---|---|---|
Platen angle | 15 degrees | 10 degrees |
Platen rotation speed | 20 rpm | 20 rpm |
Ar(N) flow | 4 sccm | 4 sccm |
Ar(dep. source) flow | 9 sccm | 8 sccm |
I(N) | 310 mA | 320 mA |
Power | 675 W | 700 W |
I(B) | 310 mA | 280 mA |
V(B) | 1200 V | 1100 V |
Vacc(B) | 400 V | 400 V |
Deposition time | 29 min | 37 min |
Other results
Roughness of the surface
Measured with the Optical profiler - PSI mode (on one sample from the acceptance test): Sa= 0.6 nm
Uniformity and break down voltage by Mathias Engholm 2016-11-29
Mathias made 105.62nm SiO2 on a test silicon wafer and on his sample wafer. The sample wafer had gold/Cr on the surface and that had to be electrically isolated. The uniformity over the wafer of the oxide was 0.19% over 9 points - this is better than he has achieved when oxidizing in a furnace. He anodic bonded the wafer without problems. He measured the breakdown voltage and got 0.82+/+ 0.13 V/nm over 24 points. This is just as good as the oxide from the furnaces. Before his deposition he ran a 20 min heat up and 40min dummy deposition to clean the target. This was done with a bright new target and with the small deposition grids mounted.